View original document

The full text on this page is automatically extracted from the file linked above and may contain errors and inconsistencies.

Alternative Metals Study
Phase II

Technical Report
2014 Biennial Report to the Congress

United States Mint
Department of the Treasury
FINAL
August 11, 2014

This page intentionally left blank.

I.

Executive Summary

The Coin Modernization, Oversight, and Continuity Act of 2010, Public Law 111-302
(CMOCA) authorizes the Secretary of the Treasury to conduct research and development on
“possible new metallic materials or technologies for the production of circulating coins.”
CMOCA also specifies that before the second anniversary of its enactment, and biennially
thereafter, the Secretary of the Treasury shall submit a report to Congress, analyzing
production costs for each circulating coin, cost trends for such production, and possible new
metallic materials or technologies for the production of circulating coins.
After Phase I concluded in December 2012, the United States Mint (Mint) delivered the first
biennial report to Congress, and then continued its research into alternative metals, rejecting
some of the materials recommended in that report, and identified six materials that would
form the major effort for continued testing in Phase II. Beyond those six compositions,
however, the Mint continued to consider and evaluate other, potential, alternative materials.
For Phase II testing, the following materials were evaluated:
Material

Composition

Tested On

1

Copper-plated zinc (CPZ)

Copper plated on zinc
(identical to current one-cent)

Five-cent

2

Tin-plated CPZ (TPCPZ)

Tin plated on copper plated on
zinc

Five-cent

3

Nickel-plated steel (NPS)

4

Multi-ply-plated steel
(MPPS)

5

Stainless steel

6

80/20 cupronickel (80/20)

Nickel plated on low-carbon
steel
Nickel plated on copper plated
on nickel plated on low-carbon
steel
Austenitic (non-ferromagnetic)
stainless steel, monolithic
80% copper, 20% nickel,
monolithic

Five-cent
Quarter-dollar*
Five-cent
Quarter-dollar
Five-cent
Five-cent**

* Materials were tested on the quarter-dollar with the intent of applying those results to the dime and half-dollar.
** 80/20 was only tested on the five-cent but was expected to be clad to copper for higher denominations if it passed.

The Mint chose the top five listed as “co-circulate” materials, meaning the Mint recognized
that the material would not have the same electromagnetic signature (EMS) or piece weight
as the material of same-denomination coins that are currently in circulation (current
material). The Mint chose 80/20 as a “seamless” material, meaning the Mint expected the

i

material to match the current material’s EMS and weight, and have no appreciable impact on
the coin-accepting industry.
The Mint purchased all materials except stainless steel in variability lots, which were
laboratory-produced and contained 500–2,000 pieces made to specifications to provide the
expected range of material properties in production. The supplier provided multiple
configurations, typically modifying the key variable such as plating thickness, to provide the
Mint with samples that would span the normal variation to be expected in production
material. Those materials that passed the variability lot testing were then purchased in preproduction lots, which were much larger, typically about 2 million pieces. Pre-production
lots were produced on the supplier’s normal manufacturing lines over separate production
runs to evaluate material that would be representative of actual production.
During variability testing, materials were processed through progression strikes to show how
varying strike force (in metric tons, or tonnes) would affect the material’s detail (“fill”) as
compared with the current coins. The Mint also put test pieces through a two-week
accelerated wear test, a steam test designed to test the material’s resistance to color change,
and various other tests, such as conductivity, hardness, and EMS. Then, the materials had to
pass a Go/No-Go determination on seven criteria.
TPCPZ and CPZ both failed their Go/No-Go determinations because of poor results on the
wear test. NPS and MPPS passed their Go/No-Go criteria for both the five-cent and the
quarter-dollar and the Mint purchased those materials for pre-production testing. As the
Mint had not finalized security requirements of the quarter-dollar at that time, it purchased
NPS and MPPS for the quarter-dollar. Stainless steel was the subject of a Feasibility Study at
the time, and had not yet reached the Variability stage as the other co-circulate materials
had.
The original 80/20 material’s EMS did not match the current material. However, a slightly
modified version of the 80/20 material, which substituted manganese for some of the nickel
to achieve the conductivity and EMS of the current material, showed promise. Accordingly,
the Mint procured about 500 pieces of this modified 80/20 to run it through the progression
strikes, wear test, and steam test. The Mint also tested the modified 80/20’s EMS at three
different external coin acceptor manufacturers that all confirmed an EMS match with the
current material. The Mint determined that modified 80/20 passed its Go/No-Go criteria
and, accordingly, it purchased additional quantities for pre-production testing.

ii

The Mint purchased NPS and MPPS in five-cent and quarter-dollar configurations and the
modified 80/20 (from this point on in the Executive Summary, referred to as “80/20”) in fivecent configuration for the pre-production testing. Initially, NPS and MPPS proved to have
poor striking qualities in the variability testing. However, the Mint consulted with The
Royal Mint (RM) and the Royal Canadian Mint (RCM), both of which have experience with
these cold-rolled 1, low-carbon, plated-steel materials, and identified various changes to
mitigate these issues. In addition, the Mint had to send nonsense dies (some polished to
ascertain the effects of die surface preparation on striking) to RM and RCM for physical
vapor deposition (PVD) coating to enable dies to withstand the severe abrasion associated
with nickel plating on both of these products.
The RM and RCM sent to the Mint quantities of both materials, which showed
improvement, but the Mint still had problems with die life and fill. After more interaction
with the RM and RCM, the Mint received pre-production lots and conducted full tests on
both plated-steel materials. The die life still proved significantly less than with the current
material. The Mint determined that noticeable changes to the coin aspects (including
adjustment to the height of relief/crown, smoothing design features, softening letters, and
less-detailed images in general) would be needed to improve coinability. In addition,
planchet profiles and blank lubrication would need optimization. The tests suggest that the
plated-steel materials will not surpass or even match the current material in coinability.
The Mint also investigated stainless steel as a co-circulate option, either as a monolithc
material for the five-cent, or as a clad material for the dime, quarter-dollar, and half-dollar.
The security requirements of the quarter-dollar (and higher denominations) make this easilycounterfeited material unsuitable for those denominations, though it would be feasible for
the five-cent. Further testing would be required to determine its feasibility for cladding the
dime.
The Mint is still researching other alternatives to the ones already tested in this report. Of
note are coins made of a variation on “nickel silver,” a material composed of copper, nickel,
and zinc that has a silver appearance. The variation, alloy C77000, is expected to yield a coin
that has the same EMS as current coins, and (similar to the 80/20 alloy) has a weight that falls
into the acceptable variation on current coins. The Mint is partnering with the National
Rolling is a metal process in which metal stock is pressed through one or more pairs of rollers to reduce the
thickness of the metal. Cold-rolled indicates that the rolling was at a temperature in which the metal grains do
not recrystallize; the absence of recrystallization reduces the material’s ability to deform under stress (ductility).

1

iii

Institute of Standards and Technology (NIST), a bureau of the Department of Commerce, to
pursue an alloy development project.
The Mint is also investigating plated coins that use a silicon-steel core, not used elsewhere in
the world, that could have a unique EMS. Silicon steel is commonly referred to as “electrical
steel” and has a similar price to low-carbon steel.
Tables I-1 and I-2, on pages vii and viii, provide a performance summary of the co-circulate
materials in the Down Selection, first for the five-cent, and then for the quarter-dollar.
The charts show that MPPS and NPS have superior durability compared with the current
material. However, MPPS and NPS were less coinable than the current material; were not as
recyclable; were more vulnerable to counterfeiting and fraud; and MPPS is only available
from the RCM, unlike the other candidate materials and the current material, which all have
multiple suppliers. This makes NPS and MPPS feasible for the five-cent, but (due to security
requirements) not feasible for the quarter-dollar.
External Studies

During the course of Phase II, the Mint contracted Concurrent Technologies Corporation
(CTC), which had conducted Phase I of the Alternative Metals Study in 2010–2012, to
evaluate the potential use of bi-metallic coin construction for U.S. coins, and to study the
feasibility of stainless steel for use in U.S. coins. The Mint also contracted Fraunhofer USA, a
company that specializes in applied research for government and industry customers, to
research laser-blanking as a production improvement at United States mints.
All three reports are attached to this report, and their executive summaries are in Sections 7
(Bi-Metallic Coins), 8 (Stainless Feasibility), and 9 (Laser-Blanking).

iv

Findings and Conclusions
Two separate types of alternatives were considered during Phase II testing/evaluation. The
first was a material with an EMS and piece weight that was potentially seamless with the
current material. The second were co-circulate alternatives in which the EMS differed from
the current material and the piece weight would vary from the current material by 4 percent
or more.
Potentially seamless alternatives would not require changes to the coin acceptors, but would
only offer modest annual savings (approximately 3 percent). Co-circulate alternatives
provide much greater annual savings (up to approximately 20 percent), but would require
significant stakeholder conversion costs to accommodate the different EMS and piece weight.
•

Potentially seamless alternative evaluated:

80/20

•

Co-circulate alternatives evaluated:

Nickel-plated steel (NPS)
Multi-ply-plated steel (MPPS)
Stainless steel
Copper-plated zinc (CPZ)
Tin-plated CPZ (TPCPZ)

Seamless Material

1. A variant of today’s current cupronickel composition, termed 80/20, which has a
lower nickel content with higher manganese, was found to be seamless when tested
by three separate coin-acceptor manufacturers. 2 The Mint estimated this material
would provide approximately $5.25M annual savings ($3.2M for the five-cent, $0.8M
for the dime, $1.25M for the quarter-dollar) with no impact on the public or on
stakeholders.
2. 80/20 matches the current material in both EMS and in piece weight, having a weight
that falls within legally accepted variances for the current material.
3. Initial testing of other, potentially seamless, leaner-copper alternatives shows
potential for further incremental material savings.

2

In testing, treated 80/20 five-cent pieces were 100% accepted by all three coin-acceptor manufacturers.

v

Co-Circulate Materials

4. Plated-steel materials are a viable option for the five-cent and potentially the dime,
and offer up to approximately $29M in savings annually over current materials.
However, plated-steel materials have increased risks of fraud and counterfeit, and are
used in low-value foreign coins, all of which make the materials not feasible for use in
the quarter-dollar. They also have a significantly lower die life, which, if not
mitigated (see #6, below), could increase production and labor costs, and reduce the
savings the materials might offer.
5. Stainless steel, while resistant to corrosion, has a hardness that can negatively impact
its coinability. Control of cold-rolling reduction and proper annealing of the right
grades demonstrated the ability to mitigate this factor, and improves the coinability of
stainless steel. (See attached Stainless Feasibility Study and its Executive Summary in
Section 8.)
Production Improvement

6. The Mint explored options of adjusting the height of the relief and crown on the
current coin design to address unacceptable fill on some materials. However, this
change introduced other issues, such as outer elements (e.g., the border) filling before
inner ones, or the flow of the material changing. It became clear that changes to the
coin features—including adjustments to the height of relief/crown, planchet profile,
smoothing of design, softening of the letters, and less-detailed images in general—
must be treated as a collective system. This system involves not only the items
mentioned here, but also matching planchet-die geometry, strike force, die
lubrication/coating/polishing, and other variables.
Terminated Materials

7. Testing of plated zinc alternatives (copper-plated zinc (CPZ) and tin-plated copperplated zinc (TPCPZ)) showed insufficient wear and durability properties for
consideration on denominations other than the current one-cent CPZ application.
Additionally, TPCPZ exhibited galvanic corrosion when copper and tin, two
dissimilar metals, were exposed to the environment during wear, rendering this
construction unsuitable for any U.S. coins.

vi

Table I-1.

Five-Cent Down-Select Summary

vii

Table I-2.

Quarter-Dollar Down-Select Summary

viii

Technical Recommendations for Further Study

1. Continue 80/20 Testing and Evaluation
a. Continue larger-scale testing of 80/20 and develop a final specification that can
be utilized by current and other strip suppliers.
b. Conduct feasibility, variability, and pre-production testing on cladding 80/20
to a copper core as an alternative for the clad denominations of dime, quarterdollar, and half-dollar. The primary benefit of this is the streamlining of the
material production.
2. Pursue seamless alloy development
Continue alloy development of other, potentially seamless, leaner-copper
alternatives to provide opportunity for additional incremental materials
savings without impacting coin acceptors and coin processors. Initial testing
indicates further opportunity for incremental material cost reductions with a
composition evolving over several progressive steps.
3. Continue stainless steel R&D
a. Continue larger-scale variability and pre-production testing on the two
stainless steel grades identified in the attached Stainless Feasibility Study:
Rittenhouse 52 and 18-9LW.
b. Conduct testing and evaluation of monolithic stainless steel as a clad outer
layer as a co-circulate material. Engineering calculations indicate this
combination could exhibit a similar EMS to the current clad coins and enable
the copper core thickness to be reduced, providing incremental material
savings and a reduction in the use of the more-expensive and price-volatile
nickel. Its piece weight, however, would be lighter.
4. Explore production improvements
a. Investigate push-back blanking and determine if that is a technically feasible
and cost-effective production method that would enable elimination of
internal annealing on strip material (see attached Laser-Blanking Study).
b. Pursue more-structured test strikes on different coin materials, modified
design aspects, and upset profile configurations to increase the Mint’s
understanding of the overall coin manufacturing system. These results can be
utilized to improve production efficiencies on current coin materials and
provide for quicker evaluation of future materials. Results from structured
trials can be used to support predictive model development and reduce the
need for time-consuming iterative test strikes.

ix

This page intentionally left blank.

x

II.

Table of Contents

I.

Executive Summary

i

II.

Table of Contents

III.

Table of Figures

xvi

IV.

Table of Tables

xvii

1.

Introduction

xi

1

1.1.

Background ...................................................................................................................... 1

1.2.

Public Law ....................................................................................................................... 2

1.3.

Costs ................................................................................................................................. 2

1.4.

Summary of Phase I ........................................................................................................ 5

1.4.1.

Alternative Metals Considered but Eliminated...................................................... 5

1.4.2.

Alternatives to Production ...................................................................................... 7

1.4.3.

Proposed Action ....................................................................................................... 8

1.5.

Phase II .......................................................................................................................... 10

1.5.1.

Introduction ........................................................................................................... 10

1.5.2.

Objective ................................................................................................................ 10

1.5.3.

Testing .................................................................................................................... 11

1.6.

Other Research and Development ............................................................................... 12

1.7.

Testing Facilities ............................................................................................................ 13

1.8.

Independent Peer Review ............................................................................................ 14

1.8.1.
1.9.
2.

Argonne Report Executive Summary ................................................................... 15

Public Law 111-302....................................................................................................... 17
Materials

2.1.

19

Introduction .................................................................................................................. 19

2.1.1.

Raw Metals ............................................................................................................. 19

2.1.2.

Other Considerations............................................................................................. 24

2.2.

Approach ....................................................................................................................... 25

2.3.

Key Features .................................................................................................................. 26

2.3.1.

EMS ......................................................................................................................... 26

xi

2.3.2.

Weight .................................................................................................................... 27

2.3.3.

Color ....................................................................................................................... 27

2.3.4.

Construction........................................................................................................... 28

2.3.5.

Hardness ................................................................................................................. 29

2.4.

The Materials ................................................................................................................. 31

2.4.1.

Current ................................................................................................................... 31

2.4.2.

80/20 Cupronickel.................................................................................................. 31

2.4.3.

Copper-Plated Zinc (CPZ)..................................................................................... 32

2.4.4.

Multi-Ply-Plated Steel ........................................................................................... 32

2.4.5.

Nickel-Plated Steel ................................................................................................ 33

2.4.6.

Stainless Steel ......................................................................................................... 33

2.4.7.

Tin-Plated Copper-Plated Zinc (TPCPZ) ............................................................. 34

2.5.

Cost ................................................................................................................................ 34

2.6.

Sourcing ......................................................................................................................... 38

3.

Testing
3.1.

39

Control Plan and Procedures ........................................................................................ 39

3.1.1.

Control Plan ........................................................................................................... 39

3.1.2.

Procedures .............................................................................................................. 39

3.2.

Steps ............................................................................................................................... 40

3.2.1.

Progression Strikes ................................................................................................. 40

3.2.2.

Testing Results ....................................................................................................... 41

3.2.3.

Wear Test ............................................................................................................... 41

3.2.4.

Steam Test .............................................................................................................. 42

3.2.5.

Coin Sorter/Validator (CSV) Test ......................................................................... 43

3.2.6.

Hardness Test ......................................................................................................... 44

3.2.7.

Electrical Conductivity Test .................................................................................. 45

3.3.

Material Tests – Variability Lots .................................................................................. 46

3.3.1.

CPZ (Variability Lot) ............................................................................................. 46

3.3.2.

Tin-Plated Copper-Plated Zinc (Variability Lot)................................................. 51

3.3.3.

Multi-Ply-Plated Steel (Variability Lot) ............................................................... 56

xii

3.3.4.

Nickel-Plated Steel (Variability Lot) .................................................................... 62

3.3.5.

Cupronickel 80/20 from Supplier A (80/20A) (Variability Lot) .......................... 68

3.3.6.

Cupronickel 80/20 from Supplier B (80/20B) (Variability Lot) ........................... 71

3.4.

Pre-Production Testing................................................................................................. 74

3.4.1.

CPZ Pre-Production Data ..................................................................................... 74

3.4.2.

Down-Selection Matrices ...................................................................................... 74

3.4.3.

Multi-Ply-Plated Steel (Pre-Production Lot) ....................................................... 80

3.4.4.

MPPS Down-Selection .......................................................................................... 83

3.4.5.

Nickel-Plated Steel (Pre-Production Lot) ............................................................ 85

3.4.6.

NPS Down-Selection ............................................................................................. 89

3.4.7.

Cupronickel 80/20B (Pre-Production Lot) ........................................................... 91

3.4.8.

80/20B Down-Selection ......................................................................................... 93

4.

U.S. Coin Security
4.1.

95

Threats ........................................................................................................................... 95

4.1.1.

Counterfeiting ........................................................................................................ 95

4.1.2.

Fraud ....................................................................................................................... 95

4.2.

Security Features of U.S. Coinage ................................................................................ 96

4.2.1.

Background ............................................................................................................ 96

4.2.2.

Variances in Conductivity/EMS ............................................................................ 97

4.2.3.

Coin Construction.................................................................................................. 98

4.2.4.

Coin Security Evolution ........................................................................................ 98

4.3.

Steel-Based Coin Security ............................................................................................. 99

4.3.1.

Plated Steel ........................................................................................................... 101

4.3.2.

Stainless Steel ....................................................................................................... 103

4.3.3.

Homogeneous Materials ...................................................................................... 104

4.3.4.

Coin Sorter/Validator Testing ............................................................................. 104

4.4.
5.

Steel-Based Coin Security Conclusions...................................................................... 106
Coinability

107

5.1.

Testing Methods .......................................................................................................... 107

5.2.

Baseline Results ........................................................................................................... 108

xiii

5.2.1.

80/20B Five-Cent ................................................................................................. 110

5.2.2.

Multi-Ply-Plated Steel (Five-Cent)..................................................................... 113

5.2.3.

Multi-Ply Plated Steel Quarter-Dollar ............................................................... 115

5.2.4.

Nickel-Plated Steel Five-Cent ............................................................................. 117

5.2.5.

Nickel-Plated Steel Quarter-Dollar .................................................................... 119

5.3.
6.

Conclusions.................................................................................................................. 123
Findings/Conclusions and Recommendations

125

6.1.

Findings and Conclusions ........................................................................................... 125

6.2.

Recommendations for Further Study ......................................................................... 128

7.

Bi-Metallic Coin Study
7.1.

129

8.

Executive Summary .................................................................................................... 129
Stainless Steel Feasibility Study

8.1.

137

9.

Executive Summary .................................................................................................... 137
Laser-Blanking Study

9.1.

139

10.

Executive Summary .................................................................................................... 139
Appendices

10.1.

147

Wear Test Results – Variability Lots ...................................................................... 147

10.1.1. Copper-Plated Zinc (CPZ)................................................................................... 147
10.1.2. Tin-Plated CPZ (TPCPZ) .................................................................................... 148
10.1.3. NPS ....................................................................................................................... 150
10.1.4. MPPS .................................................................................................................... 152
10.1.5. 80/20A (Variability) ............................................................................................. 154
10.1.6. 80/20B (Variability) ............................................................................................. 155
10.2.

Steam Test Results – Variability Lots ..................................................................... 156

10.2.1. CPZ Steam Test .................................................................................................... 156
10.2.2. TPCPZ Steam Test ............................................................................................... 157
10.2.3. NPS Steam Test .................................................................................................... 159
10.2.4. MPPS Steam Test ................................................................................................. 161
10.2.5. 80/20A Steam Test (Variability) .......................................................................... 163
10.2.6. 80/20B Steam Test (Variability) .......................................................................... 164

xiv

10.3.

Conductivity and CSV Test Results – Variability Lots .......................................... 165

10.3.1. CPZ Conductivity and CSV................................................................................. 165
10.3.2. TPCPZ Conductivity and CSV ............................................................................ 168
10.3.3. NPS (Conductivity Test Not Applicable)............................................................ 176
10.3.4. MPPS (Conductivity Test Not Applicable) ........................................................ 178
10.3.5. 80/20A (Conductivity Results Unavailable) ....................................................... 180
10.3.6. 80/20B (Conductivity Results Unavailable)........................................................ 181
10.4.

Wear Test Results – Pre-Production ...................................................................... 182

10.4.1. NPS ....................................................................................................................... 182
10.4.2. MPPS .................................................................................................................... 186
10.4.3. 80/20B ................................................................................................................... 188
10.4.4. CPZ ....................................................................................................................... 190
10.5.

Steam Test Results – Pre-Production ..................................................................... 191

10.5.1. Nickel-Plated Steel .............................................................................................. 191
10.5.2. MPPS .................................................................................................................... 195
10.5.3. 80/20B ................................................................................................................... 197
10.5.4. CPZ ....................................................................................................................... 199
10.6.

CSV Test Results – Pre-Production ........................................................................ 200

10.6.1. NPS ....................................................................................................................... 200
10.6.2. MPPS .................................................................................................................... 204
10.6.3. 80/20B ................................................................................................................... 206
10.6.4. CPZ ....................................................................................................................... 207
CSV Comparison—Plated Steel v. Current Material ............................................. 208

10.7.
11.

Acronym List

209

xv

III.

Table of Figures

Figure 1-1. Historical Unit Cost of the One Cent ......................................................................3
Figure 1-2. Historical Unit Cost of the 5 Cent ...........................................................................3
Figure 2-1. Commodity Price History of Nickel, 1999 to 2014 ...............................................19
Figure 2-2. Commodity Price History of Copper, 1999 to 2014..............................................20
Figure 2-3. Commodity Price History of Zinc, 1999 to 2014 ..................................................21
Figure 2-4. Commodity Price History of Aluminum, 1999 to 2014 .......................................22
Figure 2-5. Commodity Price History of Steel Billet, 2008 to 2014 ........................................23
Figure 2-6. Quarter-Dollar Nonsense Test Pieces ....................................................................25
Figure 2-7. Electroplating ..........................................................................................................28
Figure 2-8. Damaged Die ...........................................................................................................30
Figure 3-1. R&D Coining Press .................................................................................................40
Figure 3-2. Steam Test Tumblers ..............................................................................................41
Figure 3-3. Steam Test Autoclave .............................................................................................43
Figure 3-4. High-Speed CSV .....................................................................................................43
Figure 3-5. Hardness Tester .......................................................................................................44
Figure 3-6. CPZ Test Piece ........................................................................................................46
Figure 3-7. 5 Cent CPZ Blank Color Change—Variability Lot ...............................................47
Figure 3-8. 5 Cent CPZ Planchet Hardness Test—Variability Lot .........................................48
Figure 3-9. CPZ After Wear Test ..............................................................................................49
Figure 3-10. 5 Cent TPCPZ Blank Color Change—Variability Lot ..........................................51
Figure 3-11. Quarter Dollar TPCPZ Blank Color Change—Variability Lot ............................52
Figure 3-12. 5 Cent TPCPZ Planchet Hardness Test—Variability Lot.....................................52
Figure 3-13. Quarter Dollar TPCPZ Planchet Hardness Test—Variability Lot .......................53
Figure 3-14. TPCPZ After Wear Test .........................................................................................54
Figure 3-14. MPPS 5-Cent Test Piece .........................................................................................56
Figure 3-15. MPPS Quarter-Dollar Test Piece ...........................................................................57
Figure 3-16. 5 Cent MPPS Blank Color Change—Variability Lot ............................................57
Figure 3-17. Quarter Dollar MPPS Blank Color Change—Variability Lot ..............................58
Figure 3-18. 5 Cent MPPS Planchet Hardness Test—Variability Lot.......................................58

xvi

Figure 3-19. Quarter Dollar MPPS Planchet Hardness Test—Variability Lot .........................59
Figure 3-20. MPPS Quarter Dollar After Wear Test .................................................................61
Figure 3-21. NPS 5-Cent Test Piece ............................................................................................62
Figure 3-22. NPS Quarter-Dollar Test Piece ..............................................................................63
Figure 3-23. 5 Cent NPS Blank Color Change—Variability Lot ...............................................63
Figure 3-24. Quarter Dollar NPS Blank Color Change—Variability Lot .................................64
Figure 3-25. 5 Cent NPS Planchet Hardness Test—Variability Lot..........................................64
Figure 3-26. Quarter Dollar NPS Planchet Hardness Test—Variability Lot ............................65
Figure 3-27. NPS Quarter Dollar After Wear Test.....................................................................66
Figure 3-28. 80/20A Test Piece (54T Strike)...............................................................................68
Figure 3-29. 5 Cent 80/20A Planchet Hardness Test—Variability Lot .....................................69
Figure 3-30. 80/20A After Wear Test .........................................................................................70
Figure 3-31. 80/20B Test Piece (54T Strike) ...............................................................................71
Figure 3-32. 5 Cent 80/20B Planchet Hardness Test—Variability Lot .....................................72
Figure 3-33. 80/20B After Wear Test ..........................................................................................73
Figure 3-34. MPPS 5-Cent Test Piece (56T Strike) ....................................................................80
Figure 3-35. MPPS Quarter-Dollar Test Piece (64T Strike) ......................................................81
Figure 3-36. 5 Cent MPPS Blank Color Change—Pre-Production Lot ....................................82
Figure 3-37. Quarter Dollar MPPS Blank Color Change—Pre-Production Lot ......................82
Figure 3-38. NPS Quarter-Dollar Test Piece (66T Strike) .........................................................85
Figure 3-39. NPS 5-Cent Test Piece (Detail) ..............................................................................86
Figure 3-40. 5 Cent NPS Blank Color Change—Pre-Production Lot .......................................88
Figure 3-41. Quarter Dollar NPS Blank Color Change—Pre-Production Lot .........................88
Figure 3-44. 80/20B Test Piece (54T Strike) ...............................................................................91
Figure 3-45. 5 Cent 80/20Blank Color Change—Pre-Production Lot ......................................92
Figure 4-1. Slugs and Tokens .....................................................................................................96

IV.

Table of Tables

Table I-1.

5-Cent Down-Select Summary ............................................................................. vii

Table I-2.

Quarter-Dollar Down-Select Summary ............................................................... viii
xvii

Table 1-1.

FY2014 Unit Cost of Producing and Distributing Coins, by Denomination .........4

Table 1-2.

Eliminated Candidate Metals for Coinage ...............................................................6

Table 1-3.

CTC-Recommended 5-Cent Alternatives ...............................................................9

Table 1-4.

CTC-Recommended Dime, Quarter-Dollar, and Half-Dollar Alternatives ..........9

Table 1-5.

Average Die-Life Performance (5 Cent) – Philadelphia .......................................12

Table 1-6.

Average Die-Life Performance (Quarter Dollar) – Philadelphia .........................12

Table 2-1.

Phase II Test Program Summary............................................................................26

Table 2-3.

Current Material Specifications .............................................................................31

Table 2-4.

80/20B Specifications ..............................................................................................32

Table 2-5.

CPZ Specifications ..................................................................................................32

Table 2-6.

MPPS Specifications ...............................................................................................33

Table 2-7.

NPS Specifications ..................................................................................................33

Table 2-8.

Stainless Steel Specifications ..................................................................................34

Table 2-9.

TPCPZ Specifications .............................................................................................34

Table 2-10. Estimated Unit Costs of 5-Cent Candidates ..........................................................35
Table 2-11. Estimated Unit Costs of Quarter-Dollar Candidates .............................................36
Table 2-12. Estimated Cost Breakdown – Current and Alternative Metals ............................37
Table 4-1.

EVA Coin Value Categories .................................................................................100

Table 4-2.

Foreign Plated-Steel Coins ...................................................................................102

Table 4-3.

Counterfeit Seizures in China ..............................................................................103

Table 5-1.

Baseline Die-Life Determination (5 Cent)...........................................................109

Table 5-2.

Baseline Die-Life Determination (Quarter Dollar) .............................................110

Table 5-3.

Initial 80/20B Die Life (5 Cent) ............................................................................111

Table 5-3.

Treated 80/20B Die Life (5 Cent) .........................................................................112

Table 5-4.

MPPS Die Life (5 Cent) ........................................................................................114

Table 5-5.

MPPS Die Life (Quarter Dollar)...........................................................................116

Table 5-6.

NPS Die Life (5 Cent) ...........................................................................................118

Table 5-7.

NPS Die Life (Quarter Dollar) ..............................................................................121

Table 5-9.

Pre-Production Average Die Life ........................................................................123

xviii

1. Introduction
The United States Mint (Mint) is a bureau of the United States Department of the Treasury.
Established in 1792, the Mint is the world’s largest coin manufacturer. The principal mission
of the Mint is to mint and issue circulating coins in amounts that the Secretary of the
Treasury decides are necessary to meet the needs of the United States. Current coins in
circulation are the one-cent, five-cent, dime, quarter-dollar, half-dollar, and dollar. The
half-dollar and dollar are not currently in production for circulation, though the coins
remain legal tender.
The Mint is a self-funded agency that issues circulating coins to the Federal Reserve Banks at
face value and distributes numismatic products—including collectible coins and sets, bullion
coins, medals, and related accessories—at prices established to fully recover their costs.
1.1.

Background

Prior to 1965, the four higher denomination coins (dime, quarter-dollar, half-dollar, and
dollar) were made of a 90% silver-10% copper (Ag-10%Cu) alloy; the five-cent has been a
monolithic 3 copper-nickel (Cu-25%Ni) alloy (also known as “cupronickel”) since 1866
(except for a brief change to the composition during World War II).
In 1965, in response to dwindling supplies of silver in the U.S. Treasury, Congress passed
legislation that required the Mint to replace silver coins with coins made of the five-cent’s
cupronickel alloy that was clad to a commercially pure (99.9%) copper core. The Mint
recommended these two materials and their relative thickness in the clad formulation
because this configuration provided electromagnetic properties that matched current coins in
coin acceptors at that time. The weight of the coins was slightly different, but the new coins’
lighter piece weight had no appreciable effect on their use in vending.
The one-cent was made of a copper-zinc (Cu-5%Zn) alloy before it was changed to a copperplated zinc core in 1982, in response to the rising price of copper. Since 1983, the one-cent

3

Metals are mixed together and are inseparable without smelting.

1

has been composed of a zinc-copper (Zn-0.8%Cu) alloy core, electroplated with 8 microns 4
(8µm) of pure copper.
In 2006 and 2007, the prices of nickel and copper both rose high enough to make the onecent and five-cent cost more than their face values. Because of this, since 2007, the United
States Mint has maintained regulations, approved by the Secretary of the Treasury under
31 U.S.C. § 5111(d), prohibiting the melting, exportation or treatment of one-cent and fivecent coins.
1.2.

Public Law

On November 30, 2010, the U. S. Congress passed Public Law 111-302, the Coin
Modernization, Oversight, and Continuity Act of 2010 (CMOCA), which authorized the
Mint to research and develop alternative metals for U.S. coins. The President subsequently
approved this legislation on December 14, 2010. The intent of CMOCA is to reduce the
expense of minting coins while still keeping them secure from fraud and counterfeiting. The
act also specifies that, in recommending new metals, the Secretary of the Treasury must
consider their impact on the public and stakeholders (vending machine and other coin
acceptor manufacturers, vending machine owners and operators, transit officials, municipal
parking officials, depository institutions, coin and currency handlers, armored-car operators,
car wash operators, laundromats, and American-owned manufacturers of commercial coinprocessing equipment). A copy of CMOCA can be found in Section 1.9 of this report.
1.3.

Costs

Since 2006, both the one-cent and five-cent have cost more to produce than their face value,
as shown in Figures 1-1 and 1-2, below. Rising costs of raw materials (shown as the black
line in Figures 1-1 and 1-2) have combined with rising fabrication 5 costs to contribute to that
imbalance. Conversely, the dime and the quarter-dollar cost less than half their face value to
produce as of March 2014, though the costs of their raw materials (cupronickel clad to
copper) have also risen. Two reasons these coins’ costs are not yet above face value are their

One one-millionth of a meter, or one-thousandth of a millimeter; also called a micrometer; 1µm is roughly
equivalent to 0.00003937 inches; for comparison, an average piece of paper is 75µm thick.
5 Fabrication is the process by which the material is produced by the supplier and may include plating, cladding,
and/or alloying, and can also include the cost of rolling.
4

2

relative size vs. face value and the fact that the majority of the coins’ material (two-thirds) is
the lower-cost copper core.
Figure 1-1. Historical Unit Cost of the One-Cent
3.00¢
2.41

2.50¢
2.00¢

1.67

1.50¢
1.00¢

1.42

1.21

1.62

2.00

1.79

1.83

1.77

FY13

FY14

0.97

0.50¢
0.00¢
FY05

FY06

FY07

FY08

FY09

FY10

FY11

FY12

General and Administrative costs were not figured into the one-cent’s cost until 2011.
Raw metal costs are the black line; FY14 costs are through March 2014.

Figure 1-2. Historical Unit Cost of the Five-Cent
12.00¢

11.18
9.53

10.00¢

10.09

9.22

8.83

9.41

9.08

FY13

FY14

8.00¢
6.00¢

6.03

5.97
4.84

4.00¢
2.00¢
0.00¢
FY05

FY06

FY07

FY08

FY09

FY10

FY11

FY12

Raw metal costs are the black line; FY14 costs are through March 2014.

The costs of the one-cent and five-cent coins include more than just the material cost
because the Mint does not manufacture materials, but buys them either in rolls of metal strip
or as ready-to-strike planchets.

3

When the material is received in strip form, the Mint first punches out “blanks,” or coinsized discs from the sheet. These blanks are then sent through a furnace in a process called
“annealing,” which softens the material. After this, blanks are cleaned before the “upsetting”
step, which raises the edges of the blank. At this point, the blank is called a “planchet” and is
ready to be struck into a coin. All of these steps cost the Mint resources (electricity, water,
and tools), time, and money (wages, supplies, etc.).
When the material arrives in planchet form, the supplier has handled all those previous
steps, and all that remains for the Mint is to strike the planchets into coins (as is the case
with the one-cent). In this case, supplier fabrication costs tend to be slightly higher than
coins made from strip, as they include labor and other costs of fabrication to deliver the
material in ready-to-strike form.
Mint production costs reflect the amount of work the Mint does to produce each coin; the
least amount of work is performed on the one-cent planchets which are received ready to
strike (stamp, count, and package). The five-cent, dime, and quarter-dollar all have to be
blanked, annealed, cleaned, and upset before they can be struck into coins, and their direct
Mint production costs per coin are correspondingly higher, per unit.
In all cases, though, plant overhead costs (heating, electricity, etc.) must be considered. All
of these costs add up to what is known as the Cost of Goods Sold (COGS).

Table 1-1.

FY2014 6 Unit Cost of Producing and Distributing Coins, by Denomination

Metal Cost

OneCent
0.96

FiveCent
4.97

Mint Production

0.54

1.51

0.99

1.72

Cost of Goods Sold

1.50

6.48

3.38

7.55

General and Administrative

0.28

1.34

0.65

1.46

Distribution to FRB

0.02

0.05

0.04

0.11

1.80

7.87

4.07

9.12

Total Unit Cost

QuarterDollar
2.39
5.83

Dime

Costs are shown in cents.

In addition to the COGS, the Mint incurs costs in simply running the day-to-day operations
of Mint offices in support of the coin-making process (general and administrative costs).
6

Unit costs are FY2014 YTD through March 2014

4

Finally, the cost of distributing sold coins to the Federal Reserve Banks (FRBs) is also the
Mint’s responsibility.
1.4.

Summary of Phase I

In July 2011, the Mint awarded Concurrent Technologies Corporation (CTC) a competitively
bid contract to investigate various alternative compositions for all U.S. circulating coins. The
half-dollar, dime, and quarter-dollar all have identical compositions, and of those three
denominations, only quarter-dollar nonsense pieces were struck. In addition, testing was
performed on the one-cent and five-cent.
1.4.1. Alternative Metals Considered but Eliminated
In determining what materials are suitable for replacing the current ones, the study
considered many factors, including:

U.S. industrial base ability to supply

•

Work hardening 8

material

•

Density

Material availability, now and in the

•

Environmental impact

future

•

Toxicity

•

Process consistency at mints and metal
producers

•
•

Worker health and safety
Recyclability

•

Process capabilities and current

•

Construction (plated vs. clad vs.

•
•

capitalization at Mint facilities
•

Material prices

•
•

Material price trends
Available fabrication methods

•

Fabrication costs

•

Coin die life

•

Electromagnetic signature (EMS)

•

Wear resistance

•

Corrosion resistance

•

Color and circulation-based color

monolithic)
Security (i.e., counterfeit and fraud

•

resistance)
Coin-processing equipment (hardware
and software)

•

Blind and visually-impaired
recognition and acceptance

•

General public recognition and
acceptance

•

change
•

•

Co-circulation of current and new
coins.

Coinability (i.e., low flow stress,
adequate ductility)7

operations. Ductility is a metal’s ability to be
worked without cracking, shattering or breaking.
8 Work hardening is a material response in which
the strength of metallic minerals increases due to
permanent deformation.

Flow stress is a measure of the force required to
permanently deform a metal during forming

7

5

Consideration of all these issues makes the design and selection of a coinage material and the
associated production methods a complex, challenging task.
The periodic table contains 91 metals within it (out of 118 total elements). Very early in the
project, CTC rejected the majority of those metals from consideration as an alternative coin
material for a variety of reasons. The most common reasons were the metal’s radioactivity
(uranium, plutonium, and thorium) or toxicity (lead, cadmium, and chromium). Of the
remaining metals, CTC rejected most for their softness, potentially negative environmental
impacts, and/or negative health and safety impacts.
This early review then resulted in CTC eliminating even more potential metals, primarily for
high cost, as shown in Table 1-2.

Table 1-2.

Eliminated Candidate Metals for Coinage

Element

Element
Symbol

Beryllium

Be

Too expensive; toxic

Bismuth

Bi

Too expensive; multi-colored oxidation

Cobalt

Co

Too expensive; toxic if ingested

Molybdenum

Mo

Too expensive; health issues when metalworking

Niobium

Nb

Too expensive

Tantalum

Ta

Too expensive; rare

Titanium

Ti

Too expensive

Vanadium

V

Too expensive; environmental issues

Tungsten

W

Too expensive; too hard

Zirconium

Zr

Too expensive

Silver

Ag

Too expensive*

Gold

Au

Too expensive*

Reasons for Elimination

* - Ag and Au are used for commemorative coins and for bullion.

CTC then considered the London Metal Exchange, other sources of metal prices, and global
metal supplies to determine the best possible candidate metals and alloys from those metals
that remained (iron, aluminum, zinc, tin, manganese, etc.). They determined steel, zinc, and

6

aluminum alloys to be the leading candidates to reduce the cost of coinage by replacing
nickel and copper, either partially or wholly.
In this process, CTC selected candidate metals for each circulating denomination. Low cost
was the clear driver for the one-cent. Security and ease of transition were minor concerns
because that denomination is not typically used in vending machines or in other, nonattended, automated points of sale. For all other denominations, two general categories
identified the metals and fabrication concepts: potential for seamless transition, with modest
cost savings; and potential for non-seamless co-circulation, with significant cost savings.
The candidates for seamless transition had a similar electromagnetic signature (EMS) as the
current coins, so disruption of or cost to the vending and coin-processing industries would be
minimal. Those candidate materials for the non-seamless transition did not match the EMS
of the current materials, but were designed to have an identifiable, unique EMS of their own,
whenever possible. This was to prevent fraudulent coins from being easily produced from
readily-available metals with an EMS like the new material. The introduction of nonseamless EMS coins would also result in higher conversion costs incurred by the vending
industry and other stakeholders to accommodate co-circulation. Those impacts were
discussed extensively in Chapter Four of the CTC Final Report.
1.4.2. Alternatives to Production
In addition to the alternative metals, CTC investigated alternatives to the production

methods used by the Mint. They found that the Mint’s production techniques have been
substantially the same for the last 75 years, and, through continuous improvement, remain
quite efficient. Although newer processes exist for producing volumes of small parts (such as
plastic injection molding), there are no proven ways to more economically produce the
quantity and quality of metal stampings such as those produced by the Mint at this time. All
other mints in the world use variants of the United States Mint’s processes in making their
own coins, and the Mint remains the world’s largest producer of coined products. With
respect to production methods and processes, CTC recommended no major changes to
production, and for the Mint to continue to focus on improvement.
As a result, CTC determined that significant production or equipment changes did not need
to be considered as part of the proposed action. Instead, they focused on cost-saving changes
to the composition of the coins themselves, with any subsequent changes to production
dependent on the materials selected (such as eliminating blanking, annealing, washing, and
upsetting).
7

1.4.3. Proposed Action
Based on the testing and research performed in this phase (Phase I) of the Alternative Metals
Study, CTC found that there was no more-cost-effective alternative material for the onecent, and thus recommended that it remain unchanged.
In addressing the seamless 9 alternative options, CTC recommended that the composition of
the five-cent be replaced with one of three copper-based options: 669z, G6, or unplated
31157, or a broader material specification that focused on EMS and had broader ranges of
compositions to enable more flexibility in sourcing. They also included a recommendation
to complete additional testing on 669z-clad C110 copper for use in the dime, quarter-dollar,
and half-dollar for seamless transition.
Regarding co-circulation options, CTC found that stainless steel provided a low-cost, silverwhite choice for the 5 cent that does not require further treatment for corrosion protection.
But while ferritic stainless has a lower material cost, it requires higher striking loads (which
can lead to shorter die life) and is ferromagnetic (is attracted to magnets), which is not
suitable for most coin-processing sensors. Austenitic stainless is a better candidate as it
requires lower striking loads and is not ferromagnetic.
Stainless steel options, however, have lower security, given the relatively cheaper material
available. For austenitic stainless steels, their common EMS and conductivity readings do
not vary much by grade, and so, are prone to fraud. For ferritic stainless steels, their
inconsistent EMS associated with ferritic stainless makes them less secure and the acceptor
windows have to be widened to accommodate the variation.
The following tables, 1-3 and 1-4, list the materials identified as potential replacements for
all circulating denominations except for the one-cent. CTC recommended that further
testing and evaluation be conducted on these materials, which formed the basis for Phase II
of the Alternative Metals Study.

In Phase I, “seamless” meant a material with an EMS that matched the current coin’s EMS, to allow the new
coin to be used in vending machines without changes to the coin acceptor. Diameter and thickness remained
unchanged and weight was not a consideration.

9

8

Table 1-3.
Candidate

CTC-Recommended Five-Cent Alternatives
Composition and Notes

Multi-ply-plated steel
TPCPZ-plated zinc
669z
G6 mod
Unplated 31157

10µm Ni plated on 23µm Cu plated on 4µm Ni plated on lowcarbon steel core; provided in planchet form
3µm Sn plated on 7µm Cu plated on Zn core; provided in
planchet form
Cu-10%Zn-5%Ni-10%Mn10; lower nickel content than current
material; provided in sheet form
Cu-22%Zn-10%Ni-2%Mn; lower nickel content than current
material; provided in sheet form
Cu-31%Zn-0.5%Ni-6.5%Mn; low-nickel content; provided in
planchet form

Stainless steel

Stainless steel; provided in sheet form

Nickel-plated steel

25µm Ni plated on low-carbon steel; provided in planchet form
Sn=tin, Zn=zinc, Mn=manganese

Table 1-4.

CTC-Recommended Dime, Quarter-Dollar, and Half-Dollar Alternatives

Candidate
Multi-Ply-plated steel
TPCPZ-plated zinc
TPCPZ-plated zinc
TPCPZ-plated zinc
669z-clad C110
G6-mod-clad C110
Unplated 31157-clad C110
302HQ
Nickel-plated steel

Composition and Notes
10µm Ni plated on 23µm Cu plated on 4µm Ni plated on lowcarbon steel core; provided in planchet form
5µm Sn plated on 12µm Cu plated on Zn core; provided in
planchet form
7.7µm Sn plated on 12.7µm Cu plated on Zn core; provided in
planchet form
10.2µm Sn plated on 11.2µm Cu plated on Zn core; provided in
planchet form
Cu-10%Zn-5%Ni-10%Mn cladding; lower nickel content than
current cladding; provided in sheet form
Cu-22%Zn-10%Ni-2%Mn clad to copper (C110) core; provided in
sheet form
Cu-31%Zn-0.5%Ni-6.5%Mn clad to copper (C110) core; provided
in planchet form
Stainless steel; glued to copper as “clad” material for limited
testing
25µm Ni plated on low-carbon steel; provided in planchet form

Throughout this report, chemical element percentages are in weight percent; the balance of the composition
is the first element listed.

10

9

1.5.

Phase II

1.5.1. Introduction
In Phase II of the Mint’s Alternative Metals Study, the Mint tested five-cent and quarter-

dollar alternatives. The dime, quarter-dollar, and half-dollar have an identical composition.
The Mint determined that testing of either the dime or the quarter-dollar could be
extrapolated to the other (the half-dollar could also be extrapolated), so the Mint only struck
quarter-dollar nonsense test pieces in addition to the five-cent pieces in Phase II. The dollar
coin was not addressed in Phase II.
The Mint concentrated its efforts on six materials:
•

Copper-plated zinc

(CPZ)

•

Multi-ply-plated steel

(MPPS)

•

Nickel-plated steel

(NPS)

•

Stainless steel

•

Tin-plated CPZ

(TPCPZ)

•

Cupronickel

(80/20) 11

CTC’s recommended “potentially seamless” materials (G6 mod, 669z, and 31157) had a
distinctly yellow cast to them and did not have significant cost savings, so the Mint rejected
those for further consideration. Instead, it chose to pursue a cupronickel alloy similar to that
used in the current five-cent, dime, quarter-dollar, and half-dollar (75/25) 12, but with slightly
less nickel (80/20), to provide higher cost savings with no discernible color change.
The Mint considered CPZ and monolithic stainless, but only for use in the five-cent. The
other compositions were intended for potential use in the five-cent and the quarter-dollar
(along with the dime and half-dollar). Out of all the materials tested in Phase II, only the
80/20 alloy was a potentially seamless alternative to the current materials.
1.5.2. Objective
Section 2(a)(1) of Public Law 111-302 authorizes the Secretary of the Treasury to “conduct
any appropriate testing of appropriate coinage metallic materials within or outside of the

Department of the Treasury.” The Mint designed the Alternative Metals Study with several
While the composition is not exactly 80% copper and 20% nickel, this is an approximation and is used as the
material’s term.
12 Composition is 75% copper, 25% nickel.
11

10

goals in mind. In Phase II of that Study, the Mint’s primary goal was to conduct larger scale
testing and evaluation of the materials identified in Phase I, using the quantitative measures
developed to define the ability of identified alternative material candidates to meet the
requirements of coinage production and circulation. Ultimately, the Mint’s goal is to
compare the performance of alternative material candidates with known characteristics and
properties of current coinage materials to determine suitable replacements for those current
materials.
1.5.3. Testing
The Mint tested the candidate materials in two groups during Phase II. The first group, the

“variability” lots, was a laboratory-produced, limited run intended to identify any

shortcomings in the materials and establish the variation expected in EMS before the larger
“pre-production” lots were run. The Mint purchased these “variability lots” of the selected
material in quantities at the minimum, nominal, and maximum of the supplier’s production
control band. During the variability testing, the Mint struck 500 pieces, minimum, for each
metal; this was not enough to determine die life or modes of failure, but it was more than
sufficient to determine wear, steam corrosion, external EMS characteristics, hardness,
conductivity, and coin-sorting/verification (CSV) 13 results.
Later, in the pre-production testing, the Mint tested multiple die pairs for each candidate,
and ran those either until die failure, or when a die pair reached 500,000 strikes, whichever
came first. The purpose of the pre-production stage was to determine the materials’
production viability and provide a relative indication of expected die life, not a statistical dielife projection. To estimate actual die life would require many more test runs. The Mint
chose 500,000 strikes per die pair—as that is considered a representative die life for the fivecent and quarter-dollar denominations currently minted—and four die pairs, so as to not
pose an undue burden from a testing productivity perspective. Extended runs were
conducted on the current material with nonsense dies to validate the baseline of 500,000
strikes.
Table 1-5, below, depicts current-material, five-cent, die-life performance in Philadelphia
and supports the targeted level of 500,000 strikes as reasonable, although actual performance
averages vary.
CSV machines test many variables of coins that pass through their sensors, including ferromagnetism,
permeability, EMS, diameter, and thickness. CSVs are common in the vending-machine industry.
13

11

Table 1-5.

Average Die-Life Performance (Five-Cent) – Philadelphia
CY2011

CY2012

CY2013

CY2014TD

Obverse

521

435

537

527-704

Reverse

490

577

488

560-755

Die life is shown in thousands of strikes per die.

Table 1-6, below, shows die-life performance for the quarter-dollar in Philadelphia and
supports the targeted level of 500,000 strikes as reasonable.

Table 1-6.

Average Die-Life Performance (Quarter-Dollar) – Philadelphia
CY2011

CY2012

CY2013

CY2014TD

Obverse

503

431

640

481

Reverse

497

413

647

470

Die life is shown in thousands of strikes per die.

There is more variability in quarter-dollar die life than in the five-cent’s as each year there
are five new reverse designs for the America the Beautiful (ATB) series which affects both
the reverse and the obverse die life.
1.6.

Other Research and Development

In addition to testing and evaluating the metals above, the Mint continued researching and
considering additional alternative materials. The Mint performed secondary research with
the National Institute of Standards and Technology on another potentially seamless material,
C77000, and researched co-circulate alternatives such as zinc-aluminum alloy, silicon steel,
and plated steel provided in sheets with an exposed edge. This secondary research was
intended to continue the broader search for lower-cost alternatives, and to ensure a more
thorough and ongoing approach to the Alternative Metals Study.
C77000

C77000 is a monolithic copper alloy (Cu-27%Zn-18%Ni) that the Mint identified for its
lower nickel content compared with the current alloy and for its potentially similar EMS
signature, which can make it a seamless candidate. Also known as “nickel silver,” C77000
does not exhibit the “yellowing” tendency shown by the other copper-based alloys identified
in Phase I, which was another factor in its favor. The Mint will perform more extensive
testing on this alloy and on alloys based on it to better characterize its potential.

12

Plated Steel

The Mint looked at plated steel in sheet form. Steel is much less expensive than any other
substrate in Phase II, and the use of plated strip is a more cost-effective coating method than
plating planchets. It also has a more uniform layer which would yield more consistent EMS
readings. The principal negative is the exposed edge, which would be untreated steel and
subject to corrosion.
Silicon Steel

Silicon steel, commonly called “electrical steel,” exhibited different electromagnetic
signatures from normal or stainless steel during initial testing and the Mint regarded it as a
potential alternative to the plain steel core used in the plated materials under consideration
(MPPS and NPS). Also, if its corrosion resistance could be improved, it could be considered
as a monolithic material in lower-denomination coins.
Zinc-Aluminum

The Mint pursued zinc-aluminum alloys because test pieces made solely of zinc or of
aluminum had limitations in Phase I (zinc showed poor corrosion resistance unless coated or
plated, and aluminum was very light and presented handling issues), but a combination of
the two showed initial promise. However, in testing, the combined material still showed a
lack of acceptable corrosion resistance through various metallurgical phases that created
areas of acceptable and unacceptable corrosion on the surface. This corrosion tendency
could not be controlled with a binary zinc-aluminum alloy.
Nickel-Plated CPZ

The CPZ supplier has recently developed this alternative to its CPZ, and the Mint plans on
testing this plated material to see if it will prove to be more durable than the other zincbased materials.
1.7.

Testing Facilities

In 2011, the Mint constructed a highly secure research and development (R&D) facility
inside the Philadelphia Mint and isolated from regular circulating production. This facility’s
security ensures that materials are tested thoroughly on the same type of equipment as that
used in production, and then crushed and/or stored under U.S. Mint Police oversight until
the materials can be properly (and securely) destroyed and recycled. In this way, test pieces
were isolated from normal production material and proper controls were maintained. Later
in 2013/2014, the Mint supplemented the production capabilities of the R&D room with a
secure diagnostic lab for conducting metallurgical tests and evaluating alternative materials.
13

1.8.

Independent Peer Review

The Mint proactively elected to have an independent, outside authority review the Mint’s
research methods and processes, testing methods, and data. The Mint subsequently entered
into an Interagency Agreement (IA) with the U.S. Department of Energy (DOE), which
owns the facilities that house Argonne National Laboratory (Argonne). Under the IA,
Argonne was to conduct an independent verification and validation (IV&V) of the
Alternative Metals Study, Phase II. In this independent peer review (IPR), Argonne ensured
that the Mint’s processes, tests, and evaluations were valid and that the findings and
conclusions were supportable.
During the course of testing, the Mint provided documentation of all procedures, test data,
and analyses to the Argonne IPR team for their input. Argonne responded in timely fashion
to all data sent to them over the course of the R&D effort and identified potential gaps and
concerns that were satisfactorily answered by the Mint. In every case, Argonne verified and
validated the Mint’s efforts. In late 2014, Argonne issued their official report. The following
page contains its executive summary.

14

1.8.1. Argonne Report Executive Summary
Argonne National Laboratory provided IV&V services to the US Mint for its Alternative

Metals Study – Phase II. Services includes (1) validation of project plans, (2) review testing
and evaluation, (3) review down-selection plan, and (4) validation of the US Mint’s final
recommendations. This report is the final deliverable of IV&V service contract.

Validation of project’s plans included an initial on-site visit to the US Mint R&D facilities in
Philadelphia. Testing capabilities were reviewed and found to be adequate for performing
the planned work. Documentation relating to the experimental work was reviewed and any
deficiencies were corrected by the US Mint.
Project performance was reviewed during weekly conference calls, as well as review of US
Mint experimental data documentation provided by secure file transfer. Data generated and
provided was consistent with expectations. In addition, a second site visit was performed to
review and witness on-site testing, including wear testing.
The down-selection plan was reviewed and found to be sound. The testing regimen was
sufficient to provide discriminating data amongst the various alternative metal candidates.
The US Mint’s final recommendations are documented in its 2014 Biennial Report to
Congress. Six alternative metal compositions were evaluated. The findings and
recommendations are:
1. Continue the 80/20 alloy testing and evaluation
2. Pursue seamless alloy development
3. Continue stainless steel R&D
4. Explore production improvements
The US Mint also concluded that plated zinc metal alternatives (CPZ and TPCPZ) should be
eliminated from further consideration.
IV&V Findings Statement

The US Mint followed established protocols in performing the R&D work. The work plan
was sound and addressed the key metal physical and chemical properties. The tests revealed
positive and negative aspects of the alternative metals under consideration. The findings,
conclusions, and recommendation made by the US Mint are supported by the work
performed in this project.

15

This page intentionally left blank.

16

1.9.

Public Law 111-302

Public Law 111–302
111th Congress

An Act
To provide research and development authority for alternative coinage materials to the Secretary of the Treasury, increase
congressional oversight over coin production, and ensure the continuity of certain numismatic items.

Be it enacted by the Senate and House of Representatives of the United States of America in Congress
assembled,
SECTION 1. SHORT TITLE.
This Act may be cited as the ‘‘Coin Modernization, Oversight, and Continuity Act of 2010’’.
SEC. 2. AUTHORITY TO CONDUCT RESEARCH AND DEVELOPMENT ON ALL CIRCULATING COINS.
(a) IN GENERAL.—To accomplish the goals of this Act and the requirements of subchapter II of chapter 51
of title 31, United States Code, the Secretary of the Treasury may—
(1) conduct any appropriate testing of appropriate coinage metallic materials within or outside of the
Department of the Treasury; and
(2) solicit input from or otherwise work in conjunction with entities within or outside of the Federal
Government including independent research facilities or current or potential suppliers of the metallic
material used in volume production of circulating coins,
to complete the report referred to in this Act and to develop and evaluate the use of new metallic materials.
(b) FACTORS TO BE CONSIDERED.—In the conduct of research, development, and the solicitation of
input or work in conjunction with entities within and outside the Federal Government, and in reporting to the
Congress with recommendations, as required by this Act, the Secretary of the Treasury shall consider the
following:
(1) Factors relevant to the potential impact of any revisions to the composition of the material used in
coin production on the current coinage material suppliers.
(2) Factors relevant to the ease of use and ability to cocirculate of new coinage materials, including the
effect on vending machines and commercial coin processing equipment and making certain, to the greatest
extent practicable, that any new coins work without interruption in existing coin acceptance equipment
without modification.
(3) Such other factors that the Secretary of the Treasury, in consultation with merchants who would be
affected by any change in the composition of circulating coins, vending machine and other coin acceptor
manufacturers, vending machine owners and operators, transit officials, municipal parking officials,
depository institutions, coin and currency handlers, armored-car operators, car wash operators, and
American-owned manufacturers of commercial coin processing equipment, considers to be appropriate and
in the public interest, after notice and opportunity for comment.
SEC. 3. BIENNIAL REPORT TO THE CONGRESS ON THE CURRENT STATUS OF COIN PRODUCTION
COSTS AND ANALYSIS OF ALTERNATIVE CONTENT.
(a) REPORT REQUIRED.—Before the end of the 2-year period beginning on the date of the enactment of
this Act, and at 2-year intervals following the end of such period, the Secretary of the Treasury shall submit a
report to the Committee on Financial Services of the House of Representatives and the Committee on Banking,
Housing, and Urban Affairs of the Senate analyzing production costs for each circulating coin, cost trends for
such production, and possible new metallic materials or technologies for the production of circulating coins.

17

(b) DETAILED RECOMMENDATIONS.—In preparing and submitting the reports required under
subsection (a), the Secretary of the Treasury shall include detailed recommendations for any appropriate
changes to the metallic content of circulating coins in such a form that the recommendations could be enacted
into law as appropriate.
(c) IMPROVED PRODUCTION EFFICIENCY.—In preparing and submitting the reports required under
subsection (a), the Secretary of the Treasury shall include recommendations for changes in the methods of
producing coins that would further reduce the costs to produce circulating coins, and include notes on the
legislative changes that are necessary to achieve such goals.
(d) MINIMIZING CONVERSION COSTS.—In preparing and submitting the reports required under
subsection (a), the Secretary of the Treasury, to the greatest extent possible, may not include any
recommendation for new specifications for producing a circulating coin that would require any significant
change to coin-accepting and coin-handling equipment to accommodate changes to all circulating coins
simultaneously.
(e) FRAUD PREVENTION.—The reports required under this section shall make no recommendation for a
specification change that would facilitate or allow the use of a coin with a lesser value produced, minted, or
issued by another country, or the use of any token or other easily or regularly produced metal device of
minimal value, in the place of a circulating coin produced by the Secretary.
(f) RULE OF CONSTRUCTION.—No provision of this Act shall be construed as requiring that additional
research and development be conducted for any report under this Act but any such report shall include
information on any such research and development during the period covered by the report.
SEC. 4. MEETING DEMAND FOR SILVER AND GOLD NUMISMATIC ITEMS.
Subsections (e) and (i) of section 5112 of title 31, United States Code are each amended by striking
‘‘quantities’’ and inserting ‘‘qualities and quantities that the Secretary determines are’’.
SEC. 5. TECHNICAL CORRECTIONS.
Section 5112(u)(1) of title 31, United States Code is amended—
(1) by striking ‘‘exact duplicates’’ and inserting ‘‘likenesses’’;
(2) by striking subparagraph (C);
(3) by redesignating subparagraphs (D) and (E) as subparagraphs (C) and (D), respectively; and
(4) in subparagraph (A), by striking ‘‘of 3.0 inches’’ and inserting ‘‘determined by the Secretary that is
no less than 2.5 inches and no greater than 3.0 inches’’.
SEC. 6. BUDGETARY EFFECT.
The budgetary effects of this Act, for the purpose of complying with the Statutory Pay-As-You-Go Act of
2010, shall be determined by reference to the latest statement titled ‘‘Budgetary Effects of PAYGO Legislation’’
for this Act, submitted for printing in the Congressional Record by the Chairman of the House Budget
Committee, provided that such statement has been submitted prior to the vote on passage.
Approved December 14, 2010.

18

2. Materials
2.1.

Introduction

Several alloys the Mint chose to research in Phase II include similar metals. Those metals are
nickel, copper, zinc, and steel. Other metals are present in some alloys (such as manganese,
aluminum or tin), but in smaller percentages.
2.1.1. Raw Metals
The following are price histories and basic facts on the major raw metals that were a part of
Phase II of this study, from most expensive to least.
Nickel

Figure 2-1. Commodity Price History of Nickel, 1999 to 2014 14

The Mint began using nickel in its coins in 1857, and in 1866, the five-cent gained its 25
percent nickel composition/appearance and its popular moniker, the “nickel.” Its silverwhite color has made it a popular metal for coining since the 19th century, but its rising
price has made many countries replace it with less-expensive iron (steel) alloys in recent
years.

14

USGS information was only available through 2010, so was not used in this section.

19

Nickel’s price of just under $7/lb as of January 2014 was barely one-third that of its peak in
2007 and was about the same as it briefly was in 2004. However, its price in January 2014
was still over three times higher than it was in 1999, and it has seen fluctuations over the last
five years that pushed it as high as six times the 1999 price. The five-cent has borne the
brunt of this rising price as there is more nickel in that coin (1.20g) than in any other U.S.
coin (0.944g in the half-dollar, 0.472g in the quarter-dollar, 0.189g in the dime), because of
its construction and size.
Copper

Figure 2-2. Commodity Price History of Copper, 1999 to 2014

Copper has been in use in U.S. coins since the Mint was founded. It is also the most
conductive non-precious metal, and is used in electrical, plumbing, and food-service
industries, in addition to coining.
Copper’s price saw a similar percentage increase up to 2007 as most other metals did, but it
started earlier, and had more fluctuations. Copper is quickly rising in industrial use
worldwide, and as a result, its price rebounded after the drop in 2008, increasing back to or
above its 2007 levels. Copper’s price is still relatively low in spite of the percentage increase,
barely above $3/lb at the start of 2014. The quarter-dollar contains more copper (5.198g)
than any other U.S. coin produced for circulation (3.75g in the five-cent, 2.079g in the dime).
Two-thirds of the quarter-dollar’s construction is its pure-copper core, and its cladding is 75
percent copper.

20

Manganese

Manganese is the ninth-most-abundant metal on Earth, and is used mainly in steel
production. It has been used in American coins as far back as 1942, when it and silver were
added to the five-cent to replace the nickel content and some of the copper content during
World War II. It has also been used in the dollar coin since 2000.
Manganese is not traded on the commodities market, but pricing history from 2005 to
present is available. This pricing history is based on weekly average sales prices that are
averaged out from the multiple companies that have reported their sales figures.
The price of manganese increased to a high of more than $2.30/lb in 2007. In 2008, the price
fell to $1.42/lb. Prices fell further in 2009 to $1/lb., and while they have fluctuated over the
past five years, at the start of 2014, prices were just over $1/lb.
Zinc

Figure 2-3. Commodity Price History of Zinc, 1999 to 2014

Zinc is the fourth-most-common metal in use (behind iron, aluminum, and copper), and
world resources are estimated at 1.9 billion tonnes, with major deposits and several mines in
the United States.
Its price graph is quite similar to that of nickel, but at a far smaller scale (nickel reached a
peak price over $23/lb vs. barely over $2/lb for zinc). The percentage changes in both zinc

21

and nickel over the last 15 years, however, are remarkably similar. As of January 2014, zinc
was trading at just over $0.90/lb.
In spite of increasing demand for zinc, its price has remained relatively stable over the last
three years, thanks in large part to increasing production levels, worldwide.
Aluminum

Figure 2-4. Commodity Price History of Aluminum, 1999 to 2014

Aluminum is the second-most-abundant metallic element on Earth. Found primarily in the
form of bauxite, aluminum is cheaply extracted through the Hall-Héroult Process invented
in 1886.
Its price more than doubled between 1999 and 2007, reaching nearly $1.40/lb just before the
drop in 2008 took it to $0.60/lb. Prices recovered, peaking at about $1.25/lb in 2011, but as
of the start of 2014, its price was just under $0.80/lb.
Aluminum is still in high demand in multiple industries, so its price remains somewhat
higher than less-abundant materials, such as steel.

22

Steel

Figure 2-5. Commodity Price History of Steel Billet, 2008 to 2014

Steel was not openly traded before 2008

Technically an alloy rather than a raw metal, steel is iron mixed with 0.002% to 2.1%
carbon. Stainless steel adds more materials for corrosion resistance (including chromium and
nickel), and can be ferritic (4XX series, which is drawn to magnets) or austenitic (3XX and
2XX series, not drawn to magnets).
Steel began trading on the London Metal Exchange in 2008 at just under $0.25/lb. After a
brief surge in its price to an all-time high of over $0.45/lb, prices fell in 2008 until they hit
their low of slightly more than $0.15/lb in May 2009. In the five years since, its price has
recovered, but decreasing demand has kept its price relatively low; it was still just over
$0.24/lb at the start of 2014.
These are commodity prices for common grades of steel and are provided for illustrating
price trends; the steel used in plated-coin materials is a cold-rolled, low-carbon grade and is
higher in actual cost than “mild” steel. Stainless steel, with its additional alloying elements,
is higher yet in cost per pound.
The supply of each of the raw metals seen in Phase II is both stable and of sufficient supply
sources to warrant consideration as use in replacement candidates for current coins.

23

2.1.2. Other Considerations
Security and fraud prevention play a key role in this study; medium- to high-denomination 15
coins made of inexpensive, easily-accessed metals (or those that also make up washers and

other, cheap, coin-sized items) are at a high security risk, as “slugs” can pass for those coins in
automated transactions. Plating such coins may not provide enough security from slugging
or counterfeiting, as plating facilities, methods, and equipment are plentiful and relatively
inexpensive.
Lastly, in reporting to Congress with recommendations on alternative metals, CMOCA
requires the Secretary of the Treasury to consider as a factor that, to the greatest extent
practicable, any new coins work without interruption in existing coin acceptance equipment
without modification, and, to the greatest extent possible, include no recommendation for
new specifications for producing circulating coins that would require any significant change
to coin-accepting and coin-handling equipment to accommodate changes to all circulating
coins simultaneously (Public Law 111-302, Sections 2(b)(2) and 3(d)).
No single (or elemental) metal known, however, can provide a truly seamless interaction
with current coins and still provide cost savings. As a result, alloys, plated metals, and clad
configurations were the best approach to cost savings while still ensuring a smooth
transition.
The candidate materials’ density (and therefore the individual piece weight) often varied
from the current material, and were usually lighter as heavier alternatives tended to be more
costly. The weight variance was difficult to avoid, because in Phase I, CTC recommended
the Mint maintain the current physical dimensions (the same diameter and edge thickness),
as changing those created a significant impact on shareholders.
CTC further estimated that the costs associated with piece weight changes would be
associated predominantly with armored car carriers and bulk coin processors. A weight
change would not eliminate a material from technical consideration, but if the candidate
material’s weight varied too much from the current coin weight, the material would be
considered a “co-circulate” option, and not a “seamless” one.

According to the European Vending Association’s Handbook (used by mints worldwide as the reference for
coins and coin security), “medium” value is approximately 27-68 cents and “high” value is above 68 cents. (See
Section 4.)
15

24

The Mint chose the Phase II candidate alloys and metals with these considerations in mind,
along with availability, sources of proprietary alloys, and key features of the materials,
including the material’s color and expected durability and recyclability.
2.2.

Approach

For all materials in Phase II, the Mint purchased a “variability” lot, and then for all materials
except TPCPZ, CPZ, and an 80/20 cupronickel alloy 16, the Mint purchased a “preproduction” lot. Variability lots were lab-produced and small, usually about 500–2,000
pieces of the material. The intent was to provide material that was suitable for
characterizing key attributes such as coining, wear, electromagnetic signature (EMS), and
corrosion resistance, and to establish the expected composition variation to better
characterize the EMS of each alternative material. The pre-production lots were massproduced and representative of the properties and characteristics that would be seen in
actual Mint coining. The Mint processed upwards of approximately 2 million pieces for the
material/denomination combinations.
Figure 2-6.

Quarter-Dollar Nonsense Test Pieces

For the variability lots, the Mint
asked suppliers to give a range of
production for the materials’
construction. In the case of plated
metals, for example, the
variability was on the minimum,
nominal, and maximum levels of
plating. This provided the Mint
an understanding of the
variability in the materials and
allowed the Mint to test
alternative materials before
spending more money on them. In some cases, materials were rejected from further testing
during the variability lot steps (see below).

16

Optimization of this composition is still on-going with one of the suppliers.

25

The Mint ran the pre-production lots through the same evaluation tests to which the metals
were subjected in the variability lots, but with added tests on die life and planchet
dimensions. (The short runs in the variability lots were sufficient to determine proper diestriking force, and to get an indication of die wear, but were too small to test actual die life,
or to get a true indication of planchet-size variances.)
The tests run during pre-production testing also gave the Mint a larger, more representative
sample of material results than in the variability lots, enabling an assessment of the potential
supply chain. With a broader range of test results, more accurate analysis was possible, and
the Mint gained a deeper understanding of the feasibility of candidate materials.

Table 2-1.

2.3.

Phase II Test Program Summary

Key Features

2.3.1. EMS
The electromagnetic signature (EMS) of a coin is extremely important. Most coin-accepting

machines use the coin’s EMS to verify the coin’s value and accept or reject coins on this basis.
The security of a unique EMS serves to prevent nearly-worthless discs of cheap metal (slugs)
from being passed off as genuine coins in these machines. It also prevents counterfeiters
from manufacturing their own coins from cheaper materials.
Plating provides some security and yields an EMS that is more difficult to match with
common metals, but plating can be easily replicated.
26

Cladding 17, on the other hand, can provide a coin with an EMS that is more difficult to
match inexpensively, and is not easily copied, effectively deterring counterfeiting and fraud.
2.3.2. Weight
The new coins should weigh as close as possible to the weight of current coins, as some

commercial stakeholders rely on weight to facilitate commerce. Currently, there is a +/2.1–3.2 percent variance seen 18 in U.S. coinage. This variation is accepted by coin handlers
and armored car companies as it is very minor and goes both up and down, so it tends to
balance out, overall. The Mint considers matching-EMS candidate materials with weight

that falls within this variance to be seamless.
Historically, the dime, quarter-dollar, and half-dollar have shared a direct relation between
their values and their weights. The quarter-dollar (2.5 times the value of the dime) weighs
precisely 2.5 times the weight of the dime (5.670g v. 2.268g) and the half-dollar (2.0 times
the value of the quarter-dollar) weighs exactly 2.0 times the weight of the quarter-dollar
(11.340g v. 5.670g). As a result, carriers have been able to bag dimes and quarters together
and accurately estimate their value very quickly.
If there is only a minor difference in piece weight between a candidate material and the
current material, it could be accepted as the present variation is, or the Mint could mitigate
it by making small changes in the features of the coin, and the Mint kept this in mind as
testing proceeded.
According to CTC’s report from Phase I, a change in piece weight carried a lower cost to
coin stakeholders than did a change to either the EMS or ferromagnetism of the current coin
(given that dimensions of diameter and thickness need to remain the same), but it is a peryear cost.
2.3.3. Color
Since the 19th century, the five-cent, dime, and quarter-dollar have had a silver-white

appearance. When these coins were changed to their current cupronickel composition in
1965, color was a factor in the material chosen, to allay any public concerns about the new
coins.

17
18

Cladding is defined in Section 2.3.4.
Actual figures from Philadelphia Mint production from June 2013 to June 2014.

27

CPZ was the only metal examined in the primary testing and evaluation of Phase II that is
not gray- or silver-white, and was considered solely for the five-cent based on potential cost
savings. Several alternative metal candidates in Phase I were rejected from Phase II because
they were too yellow.
2.3.4. Construction
In Phase II, the Mint examined alternative metals in three basic composition types: plated,

monolithic, and clad. No material tested in this phase was a simple elemental metal.
Plating

Plated metals have a metal core plated with one or more other metals in thin layers. The
reason for this plating can be for color, security, EMS, corrosion/wear protection, or a
combination thereof. Plating is performed in many ways, with multiple variations, but only
electroplating was seen in plated candidate metals of Phase II.
Figure 2-7. Electroplating

“Me” in this figure is a stand-in for any metal.

Electroplating uses an electric current to move metal from an anode (such as copper) in an
electrolytic solution onto a metal cathode (for example, zinc discs) in the solution. As shown
in Figure 2-7, when the anode is positively charged, its metal atoms are oxidized, creating
metal ions (Cu2+) that dissolve in the electrolytic solution. At the negatively-charged
cathode, the dissolved metal ions in the electrolytic solution are reduced to elemental metal

28

(Cu) at the solution/cathode interface. The cathode is sometimes referred to as a “core” or
“substrate.”
Plating thickness varies over the surface of the piece with heavier thicknesses on the edge, as
a function of the plating physics. This variation in plating thickness contributes to a varying
(“wider”) EMS on plated coins. When plating thicknesses are given, they refer to a
measurement in the center of the plated piece.
Monolithic

A monolithic alloy is a homogeneous (evenly mixed) blend of a metal and at least one other
material. This is different from plating or cladding in that there are no layers; the materials
are melted down and mixed together into a single alloy that is the same, through and
through.
Cladding

Clad metals can use either, both, or none of the above constructions. Cladding bonds
dissimilar metals together. The clad material could then be plated, but this is not usually
done in coining.
Typically, clad coinage metals are “roll clad,” a process in which the layers of metal (for
coins, this is usually a symmetrical “sandwich” of an odd number of layers) are thoroughly
cleaned and passed through a series of rollers under sufficient mechanical pressure to bond
the layers together. The high force serves to permanently deform the metals and to reduce
their combined thickness in the process.
2.3.5. Hardness
Rockwell 15T hardness tests determine a material’s hardness relative to other materials.

Planchets made from harder materials will typically require more force to strike or form a
coin. More force to strike can also mean more stress-induced cracking and chipping on the
die (tooling) surfaces, which creates defects on the resultant coin and can shorten the die’s
life.

29

Figure 2-8. Damaged Die

Die 00581A (obverse), with a hairline crack at the top of Martha Washington’s bonnet.

A material that is too soft, however, can excessively deform when it is blanked (cupping) 19 or
upset. Beyond the impact to production, coins made of material that is too soft can cause
significant damage to automatic coin handling/processing equipment (for example, if the
coins can cold-weld together or if they fail to convey through coin acceptors). They may
also not stand up to the wear a coin experiences in normal circulation, and can rapidly
become too damaged to circulate.
Another consideration with regards to hardness is a material’s ductility and tensile strength.
A ductile material “flows” in the striking process, allowing it to more easily fill in the peaks
and valleys in the die’s design.
While a material that shattered upon striking would have been eliminated from
consideration, no such conditions existed in Phase II, and hardness itself was not a basis in
19

See attached Laser-Blanking Study for section on “push-back blanking” as a counter to cupping.

30

determining a material’s feasibility. Ductility was, however, indirectly a factor, as it affected
how well a material achieved proper detail (“filled”) on strikes during progression strikes (the
first step in testing). As a result, the Mint considered hardness as a property to test, but not
as a precursor to success in coining a material.
2.4.

The Materials

Following are the current material used in U.S. coins, and the six candidate materials from
Phase II. These entries show only the five-cent and the quarter-dollar, as the quarter-dollar
served as the proxy for the three clad denominations (dime, quarter-dollar, and half-dollar
which use the same composition of material, just rolled to different thicknesses) for this
study.
2.4.1. Current
The Mint performed identical tests on the current material and the alternative candidates.

Table 2-3.
Coin
Five-Cent
Quarter-Dollar

Current Material Specifications

Material
Cu-25%Ni
(cupronickel)
Cupronickel clad
to copper core

Construction

Weight

Monolithic

5.000g

Clad (cupronickel over C110 copper)

5.670g

2.4.2. 80/20 Cupronickel
The 80/20 candidate is very similar to the current 75/25 material, with 20 percent less nickel
in its composition. In the five-cent, this is a significant change, though for the quarter-

dollar, it only comes to 20 percent of 8.33 percent, or only 1.67 percent of the coin’s overall
makeup. As a result, while 80/20 is a seamless alternative, cost savings with that material are
small compared with other alternatives.
The two “80/20” material samples were ordered in two different compositions; 80/20A was
Cu/20%Ni with a minor amount of manganese (which tested as having an EMS too different
from the current material), while 80/20B contained more manganese, replacing some of the
copper and nickel, for a final composition of Cu-19.7%Ni-3.3%Mn.

31

Table 2-4.

80/20B Specifications

Coin

Material

Construction

Weight

Five-Cent

Cu-20%Ni-3%Mn

Monolithic (cupronickel)

4.96g

2.4.3. Copper-Plated Zinc (CPZ)
The planchets used in the current U.S. one-cent are zinc discs plated with 8µm of copper,
known as copper-plated zinc, or CPZ. The Mint examined this material as a potential

alternative for the five-cent, but after it failed the variability lot wear test, it was dropped
from consideration.

Table 2-5.

CPZ Specifications

Coin

Material

Construction

Weight

Five-Cent

8µm Cu plated
on Zn-.8%Cu core

Zinc plated with copper

4.06g

2.4.4. Multi-Ply-Plated Steel
Multi-Ply-Plated Steel (MPPS) is a process developed and patented by the Royal Canadian
Mint (RCM) in which RCM takes a core of cold-rolled, low-carbon steel and first plates it

with nickel, then copper, and then nickel again. MPPS is used in over 60 countries; Canada
supplies approximately half of those countries with MPPS, and the other half manufacture it
under license.
The multiple layers of plating allow RCM to alter the EMS of the coin by changing the
thickness of the plating layers. The Mint struck this candidate in five-cent and quarterdollar nonsense pieces.
MPPS has significant vulnerabilities to fraud and counterfeiting, and is used in lower-value
world coins that are a similar size as the quarter-dollar, and is therefore not feasible for use in
the quarter-dollar. It is, however, feasible for use in the five-cent and potentially in the
dime.

32

Table 2-6.
Coin
Five-Cent
Quarter-Dollar

Material
4µm Ni on 5µm
Cu on 10µm Ni
on Steel core
4µm Ni on 23µm
Cu on 10µm Ni
on Steel core

MPPS Specifications
Construction

Weight

Plated (nickel-copper-nickel over
steel)

4.37g

Plated (nickel-copper-nickel over
steel)

5.03g

2.4.5. Nickel-Plated Steel
Nickel-plated steel (NPS) can be legally manufactured by anyone with the means to plate
nickel on steel. Currently, it is used on coins in the UK and a number of other countries

around the world (in 2013, the RM produced 2.29 billion NPS coins and blanks for 38
customers). NPS is made from cold-rolled, low-carbon steel planchets plated nominally with
25µm of nickel, which is thick enough to generate a clearly discernable EMS, though it is a
different EMS from current U.S. coins. The Mint struck this candidate in five-cent and
quarter-dollar nonsense pieces.
NPS has significant vulnerabilities to fraud and counterfeiting, and is used in lower-value
world coins that are a similar size as the quarter-dollar, and is therefore not feasible for use in
the quarter-dollar. It is, however, feasible for use in the five-cent and potentially in the
dime.

Table 2-7.
Coin
Five-Cent
Quarter-Dollar

Material
25µm Ni plated
on Steel core
25µm Ni plated
on Steel core

NPS Specifications
Construction

Weight

Plated (nickel over steel)

4.40g

Plated (nickel over steel)

5.03g

2.4.6. Stainless Steel
Stainless steel is more expensive than carbon steels, but it does not need surface treatment for
corrosion protection and is still priced lower than most other metals and alloys. By

definition, stainless steel contains more than 12 percent chromium, though it can contain
other elements—most notably, nickel.

33

Ferritic (i.e., drawn to magnets) stainless steel has relatively low or no nickel content, which
makes it a low-cost option over austenitic (i.e., not drawn to magnets) stainless that contains
significant quantities of nickel.
The makeup of stainless steel, while imparting the desired corrosion resistance, also makes
the material more difficult to strike. The focus of CTC's study was to identify a composition
and thermal mechanical practice 20 that provided the desired balance between the two.
The Mint, working with CTC, evaluated this easily counterfeited material solely for the lowdenomination five-cent.

Table 2-8.

Stainless Steel Specifications

Coin

Material

Construction

Weight

Five-Cent

Fe-C-Mn-Si-Ni-Cr

Monolithic Stainless Steel

4.37g

2.4.7. Tin-Plated Copper-Plated Zinc (TPCPZ)
TPCPZ is a copper-plated zinc planchet that is further plated in tin for the silver-white color

the public expects on the five-cent, dime, and quarter-dollar. The Mint struck this candidate
in five-cent and quarter-dollar nonsense pieces. TPCPZ failed the wear test, and the Mint
eliminated it from further consideration.

Table 2-9.

2.5.

TPCPZ Specifications

Coin

Material

Construction

Weight

Five-Cent

Zn-Cu-Sn

Sn plated on Cu plated on Zn

4.1g

Quarter-Dollar

Zn-Cu-Sn

Sn plated on Cu plated on Zn

4.54g

Cost

As has been stated, the driving factor behind Public Law 111-302 was lowering the cost of
U.S. coins. Production, fabrication, and metal costs all add up, but recycling options have
also been a factor, including web scrap recycling options, in the case of material sent to the
Thermal mechanical practice refers to the cold-rolling reduction and annealing practices which control the
mechanical properties of the material.
20

34

Mint as coiled roll. The cost of minting coins is defrayed when old coins and condemned
material are directly recycled by the supplier into new material for coins. When this is not
an option, however, the Mint can still see some returns if there is another recycler interested
in buying the scrap metal or if the supplier has other uses for the metal. This recycling then
introduces another security factor (ensuring the coins are melted down by the recycler) and
generally gains the Mint less money than if the material can be returned directly to the coin
material supplier and reused as stock for future coin material.
Stainless steel, CPZ, and 80/20 have direct recycling options with the coin material supplier.
These are figured into the metal costs of these materials, shown in Tables 2-10 and 2-11,
below. The cost breakdown includes estimations of fabrication costs in some cases, as the
actual numbers were not supplied.

Table 2-10.

Estimated Unit Costs of Five-Cent Candidates

Current (FY2014)

4.21

0.76

U.S. Mint
Direct
Production
0.42

80/20 Cupronickel

3.88

0.76

0.42

5.07

2.48

7.54

3XX Stainless Steel

2.11

0.76

0.49

3.35

2.48

5.83

Candidate Material

Metal
Supplier
Cost Fabrication

Metal
Overhead
+Fabrication
+G&A
+Production +Distribution
5.39
2.48

Est.
TOTAL
7.87

Multi-Ply Plated Steel

2.81

0.21

3.02

2.48

5.50

Nickel-Plated Steel

3.42

0.21

3.63

2.48

6.11

Copper-Plated Zinc

1.70

0.21

1.91

2.48

4.39

Tin-Plated CPZ

1.97

0.21

2.18

2.48

4.66

Green indicates a “seamless” alternative and red, a canceled alternative. All costs are in cents.
Plated materials’ Metal Cost and Supplier Fabrication are supplier quotes from October 2013.
All other figures are from FY2014 (YTD through March 2014).

35

Table 2-11.

Estimated Unit Costs of Quarter-Dollar Candidates

Current (FY2014)

4.08

1.75

U.S. Mint
Direct
Production
0.48

80/20 Cupronickel

3.88

1.75

0.48

6.19

2.81

9.00

Candidate Material

Metal
Supplier
Cost Fabrication

Metal
Overhead
+Fabrication
+G&A
+Production +Distribution
6.31
2.81

Est.
TOTAL
9.12

Multi-Ply Plated Steel

3.46

0.24

3.70

2.81

6.51

Nickel-Plated Steel

3.71

0.24

3.95

2.81

6.76

Tin-Plated CPZ

3.79

0.24

4.03

2.81

6.84

Green indicates a “seamless” alternative and red, a canceled alternative. All costs are in cents.
Plated materials’ Metal Cost and Supplier Fabrication are supplier quotes from October 2013.
All other figures are from FY2014 (YTD through March 2014).

Table 2-12, below, shows the cost breakdown of the current coins and their alternatives with
estimated savings.

36

Table 2-12.
5¢
FY13 5¢ 1,123 M Coins
FY14 5¢ (75-25) -->3/31/14 492M coins
80-20Cu-Ni Solid
Multi-Ply plated steel (p)
3XX Stainless steel (s)
Nickel plated steel (p)
CPZ (p) 8 µm
Tin plated CPZ (p)

Estimated Cost Breakdown – Current and Alternative Metals

Annualized
Volume

Weight
(grams)
5.00
5.00
4.96
4.37
4.46
4.40
4.06
4.10

984 M

Weight
10¢
FY13 10¢
FY14 10¢ (92-8) -->3/31/14 825M coins
80-20 Cu-Ni Clad
Multi-Ply plated steel (p)
Nickel plated steel (p)
25¢
FY13 25¢ 1,062 M Coins
FY14 25¢ (92-8) -->3/31/14 592.2M coins
80-20 Cu-Ni Clad
Multi-Ply plated steel (p)
Nickel plated steel (p)
Tin plated CPZ (p)

Notes:
a = FY13 Actuals
b = FY2014 10/1/13–3/31/14
e = Estimate
q = Supplier quote

Annual Volume (grams)
2.27
1,650 M
2.27
2.00
2.00
Weight
Annual Volume (grams)

1,062 M

5.67
5.67
5.66
5.03
5.03
4.54

Metal
Cost

$0.0530
$0.0421
$0.0388
$0.0281
$0.0211
$0.0342
$0.0094
$0.0197
Metal
Cost

$0.0204
$0.0169
$0.0165
$0.0217
$0.0225
Metal
Cost

$0.0465
$0.0408
$0.0396
$0.0346
$0.0371
$0.0379

Metal + Supplier Fab

USM O/H+

Total

+ USM Direct

G&A +

Unit

$
$
$
$
$
$
$
$

Production
0.0662
0.0539
0.0507
0.0302
0.0335
0.0363
0.0191
0.0218

Distribution
$ 0.0279
$ 0.0248
$ 0.0248
$ 0.0248
$ 0.0248
$ 0.0248
$ 0.0248
$ 0.0248

$
$
$
$
$
$
$
$

Cost
0.0941
0.0787
0.0754
0.0550
0.0583
0.0611
0.0439
0.0466

Metal + Supplier Fab

USM O/H+

Total

+ USM Direct

G&A +

Unit

Production
$
0.0307
$
0.0267
$
0.0262
$
0.0231
0.0238
$
Metal + Supplier Fab

Distribution
$ 0.0149
$ 0.0140
$ 0.0140
$ 0.0140
$ 0.0140
USM O/H+

+ USM Direct
$
$
$
$
$
$

Production
0.0714
0.0631
0.0619
0.0370
0.0395
0.0403

$
$
$
$
$

G&A +
Distribution
$ 0.0336
$ 0.0281
$ 0.0281
$ 0.0281
$ 0.0281
$ 0.0281

Cost
0.0456
0.0407
0.0403
0.0371
0.0379
Total
Unit

$
$
$
$
$
$

Cost
0.1050
0.0912
0.0900
0.0651
0.0676
0.0684

% Savings

-16.4%
-4.1%
-30.1%
-25.9%
-22.3%
-44.2%
-40.8%

Savings Compared to
YTD FY-14 5¢
Notes
through March 2014
984 M Coins
$
a
15,189,203
$
b
3,211,103
$
e
23,335,468
$
q
$
20,097,771
e
$
17,310,451
q
$
34,254,534
q
31,614,856
$
q
Savings Compared to

% Savings

-10.7%
-1.2%
-8.9%
-7.0%
% Savings

-13.2%
-1.3%
-28.6%
-25.8%
-25.0%

YTD FY-14 10¢
through March 2014
1,650 M Coins
$
a
$
8,027,772
b
$
791,839
e
$
5,956,892
e
$
4,735,956
e
Savings Compared to
YTD FY-14 25¢
Notes
through March 2014
1,062 M Coins
$
a
$
14,715,198
b
$
1,252,998
e
$
27,718,074
q
$
25,020,594
q
$
24,171,079
q

Assumptions:
> FY13 unit cost data is from FY13 Annual Report
> Mint Production, G&A, and distribution costs are FY14 YTD through March
> Volumes are annualized FY14 (YTD through March) volumes.
> Savings are calculated based on FY14 YTD through March total unit costs
and volumes

Key:
(cs)=clad strip
(p)=plated
(s)=strip
Green=seamless alternative and Red=cancelled alternative

37

2.6.

Sourcing

The Mint requires a consistent supply of metal for its coins and medals. Successful candidate
materials must therefore be made of metals that are readily available and in good supply.
This was evident when the U.S. Treasury saw its silver reserves drop to dangerously low
levels in the early 1960s.
Competition among suppliers can help the Mint keep costs down if the Mint uses materials
with multiple suppliers over those with a single, proprietary supplier. The availability and
ease of sourcing, though, must be balanced with concerns over broad access and security.
Currently, the Mint orders its materials from domestic suppliers. Suppliers get the best
quality metal at the best prices, which often means foreign sources. Those foreign sources
usually have friendly relations with the U.S., but domestic suppliers are preferable, not only
for the lower risk, but also for lower shipping costs and a shorter supply chain.
Cupronickel (80/20)

The two cupronickel suppliers for Phase II obtain their nickel and copper from many of the
same sources globally. These foreign and domestic sources have been consistent, and more
sources, including a potential domestic nickel source, are appearing.
Copper-Plated Zinc and TPCPZ

The CPZ supplier obtains its zinc primarily from Canada, but also through recycling. Its
copper and tin come from domestic and foreign sources, depending on price levels and
availability, and also from recycling.
Multi-Ply-Plated Steel

The Mint bought this material from the Royal Canadian Mint, which patented and
manufactures this material for their own and other nations’ coins.
Nickel-Plated Steel

The Royal Mint obtains their nickel and steel from sources in Wales (UK) and supplied this
material to the Mint for Phase II.
Stainless Steel

The suppliers obtain their raw materials from multiple sources, both domestic and foreign,
and in major part from recycling. Depending on which grade would be selected, there may
be sourcing limitations posed by intellectual property rights.

38

3. Testing
The Mint purchased the candidate materials first in small variability lots, typically 500 to
2,000 pieces produced in a lab environment spanning the expected range of composition/
construction anticipated in normal production processes, and tested each for the feasibility of
their use as U.S. coins. After evaluation and passing a “Go/No-Go” determination, materials
were tested in pre-production lots, typically 2 million pieces, for a final determination.
Stainless steel, however, was not run through variability or pre-production, though CTC and
the Mint tested and evaluated various, preliminary grades until two were recommended (see
the attached Stainless Feasibility Study; the Executive Summary is in Section 8). Future
testing on the two, identified, stainless-steel materials would conform to the control plan for
variability lots, and—if justified—pre-production testing.
In all cases, these materials were struck as “nonsense” pieces that, at first glance, looked like
U.S. coins with accurate dimensions, but with Martha Washington’s profile on the obverse
and had the letters in all the words (like “Liberty” or “United States of America”) scrambled.
After testing, nonsense pieces that were no longer required were crushed and either sent
back to the supplier (current baseline pieces), or securely melted (alternative metal pieces).
3.1.

Control Plan and Procedures

3.1.1. Control Plan
Before testing in Phase II began, the Mint prepared a plan by which testing would progress.

The Control Plan detailed each step in testing, the criteria “Go/No-Go,” and the assumptions,
risks, and roles and responsibilities. By creating a detailed plan, the Mint prepared a guide by
which Argonne National Lab (Argonne) could follow the Mint’s progress easily for its
Independent Peer Review (IPR) (see Section 1.8).
3.1.2. Procedures
To ensure consistent test results, the Mint established quality assurance Standard Operating

Procedures (SOPs) for each step in the testing. These SOPs established test objectives and

clearly defined, possible-result parameters. Each SOP established what kind of instrument
would be used, how long the test would last, how many pieces would be tested, and what (if
any) criteria there would be for Go/No-Go or for down selection. Throughout Phase II, the
Mint followed the SOPs, documented their progress, and provided copies of the progress
documentation and the SOPs to Argonne for its IPR.

39

3.2.

Steps

3.2.1. Progression Strikes
Each material needed to first go through “progression” strikes. The Mint first struck five

planchets of the material at a low tonnage (press force) and then examined the struck pieces
for dimensions and for image detail. The Mint then struck five more planchets at each
progressively higher tonnage, and continued to examine the dimensions and detail until it
was determined to be sufficient for a U.S. circulating coin. At each step in this process, for
each metal, the Mint recorded the tonnage, dimensions, and the level of detail.
Figure 3-1. R&D Coining Press

The horizontal press at the testing facilities.

When the correct level of detail was reached, or when the maximum tonnage for that
material was reached, the rest of the material was struck at that tonnage for that stage of
testing.
Determining “acceptable” detail fill was subjective, but was consistent throughout the testing
process. Mint engineers who were assigned to the technical team routinely conduct
progression strikes in the course of their day-to-day duties, and their extensive experience
enabled the subjective R&D assessments to be consistent.
40

3.2.2. Testing Results
Before variability testing began, the Mint set up an electronic database with minimum and

maximum acceptable dimensional results to make it easier to see if a material passed or failed
the test, and by how much. The setup also enabled the Mint to readily see the variances
within each material and judge if the material were too inconsistent. For each material, the
Mint used calibrated micrometer gauges connected to a computer to enter the relevant data

into the database where the Mint could analyze it.
For the variability lots, the Mint used a specific dimensional data system, which generated
reports for each material that showed the minimum and maximum acceptable numbers; the
average, low, and high scores for each test; and a bar chart that showed the variances in the
tests (typically a bell curve was seen).
For pre-production lots, the Mint used a software spreadsheet program to record results from
micrometers connected to the computer and generate reports that made individual points of
data easier to access.
3.2.3. Wear Test
For each material, the Mint took either one group (variability) or four groups (pre-

production) of five random pieces from test strikes and put them through a two-week-long
comparative wear test. Nonsense pieces were placed in a towel-lined tumbler with current
coins and then tumbled with a light application of artificial sweat at 40–52 °C in a humidified
environment.
Figure 3-2. Steam Test Tumblers
The facility had multiple tumblers, each
with two test compartments which were
lined with pleated towels. The towels
overlapped slightly, introducing an
occasional flip in the movement of the
pieces and coins in the tumbler. Large,
infrared lamps were placed above each
tumbler to heat the tumblers above the
condensation point of the humidified air.
Into each compartment went five sample
nonsense pieces (five-cent or quarter-dollar) of a test material, along with one each of a

41

current one-cent, five-cent, quarter-dollar, and dollar, for a total of nine pieces in each
compartment. All coins and test pieces were thoroughly cleaned before testing, and were
subsequently cleaned before each measurement. Testers wore powder-free rubber gloves
when handling the cleaned coins and test pieces.
The Mint measured the weight of each test piece before the wear test, once during the test,
and finally at the end of the test. Edge thickness of test pieces was measured before the wear
test and at the end of the test to judge deformation as compared with current material coins
of the same denomination. Those same-denomination coins had been put through the same
test previously to provide a baseline for weight loss and edge deformation. The Mint
measured weight and thickness to the fourth decimal point, in grams for the weight and in
inches for the thickness.
This was an accelerated wear test that replaced an earlier test the Mint used in Phase I. In
the earlier test, there were various other materials (leather, cork, cloth) co-mingled with the
test pieces and a larger amount of artificial sweat. The Mint determined the earlier test was
too aggressive and not representative of actual use, especially when wear-testing plated
materials. The Mint developed this optimized test procedure to address the aggressiveness
noted in Phase I of the original test.
Note that this wear test was designed to be comparative (evaluate an alternative material as
either better, the same or worse than the current material) and not to predict actual coin life.
To pass the Go/No-Go determination for the variability lot stage, candidate materials could
only lose up to twice as much weight on a percent basis as the current material lost after the
two weeks were up (i.e., exhibited at least half the life), and had to show as much
dimensional durability (keep the same edge thickness), with no more than a 0.010”
difference with the current coins tested previously.
3.2.4. Steam Test
The Mint took a small number of random blanks for each material and measured the color

(brightness and hue) with a spectrophotometer that gave a positive “L” value for the

brightness, and then an “a” value (positive for red, negative for green) and a “b” value
(positive for yellow, negative for blue) for the hue.

42

Figure 3-3.

Steam Test Autoclave
When those scores were recorded, the
Mint steamed the blanks in an autoclave
at 100 °C, atmospheric pressure, and 100
percent humidity to accelerate the
oxidation rate compared with ambient
conditions.
After this, the Mint measured the color
again and recorded the difference. Note
that this method was only used to
evaluate the properties of the chemical

layer formed during the blank preparation process. In the a and b color plan, less change
meant a better protective chemical layer.
The Mint examined the tested samples under appropriate lighting for discoloration or spots.
3.2.5. Coin Sorter/Validator (CSV) Test
Many retail, public transit, financial institutions, and other industries that handle large

numbers of coins use coin sorter/validator systems from numerous manufacturers. These
systems take many different readings of a coin to determine the coin’s diameter, edge
thickness, conductivity, and permeability, among other characteristics. For Phase II, the
Mint obtained a high-speed CSV for its R&D program.
Figure 3-4. High-Speed CSV
During variability lots, for each material, the
Mint chose random samples of no less than
100 nonsense pieces at each of the supplier’s
minimum, maximum, and nominal platings,
thicknesses, etc. During pre-production lots,
the Mint chose at least two large samples of
approximately 30,000 pieces for each material
and selected at least 100 pieces from each
subsequent sampling of 30,000 pieces.

43

The Mint then sent these pieces through the CSV to determine the material’s measurements
and electromagnetic characteristics, consistency across batches, and match with the current
material.
To ensure that the data was accurate and reliable, the Mint kept the CSV properly calibrated
at all times.
3.2.6. Hardness Test
The Mint tested a random sample of each material using a hardness tester. Blanks that were

not yet annealed and ready-to-strike planchets were both tested, and so, there are “pre-

annealed” and “annealed” results from this test, though some materials only have a score in
one of the fields (i.e., a material that could not be annealed, or a material that came already
annealed). The Mint used the Rockwell 15T scale for this test.
Figure 3-5.

Hardness Tester
The test involved putting a planchet in the
hardness tester, and applying a minor load
to the material, which established the
“zero position.” A major load was then
applied and removed, leaving the minor
load in place. The tester then showed the
depth of penetration from the zero
position, on a readout in which harder
materials have a higher number. For small
lots (30 or fewer), each piece was tested in

five different points, with the highest and lowest of the five readings disregarded. The Mint
then averaged the remaining three readings for that piece’s reading. For larger lots (over 30
pieces), the Mint took one reading per piece, and performed statistical analysis on the data
sets, using them for comparison and evaluation.
Nominal hardness values for current materials are between 62 and 72 21, and this was the
target for the candidate materials, but hardness was not a consideration for Go/No-Go.

21

The Rockwell hardness number is relative, with no unit.

44

3.2.7. Electrical Conductivity Test
Conductivity is the measure of how well a material carries an electrical charge. Copper is the
most conductive non-precious metal, and is used as the standard for conductivity. In 1913,
due to a lack of uniformity in the value of annealed copper in various countries, the U.S.
National Bureau of Standards (now the National Institute of Standards and Technology)
developed the International Annealed Copper Standard (IACS) which was quickly adopted
by the International Electrotechnical Commission. This standard was accepted by 1914 and
is still used.
The IACS uses a percentage score to represent the conductivity of a metal. A score of 100
percent IACS translates to 58 million siemens 22 per meter at 20 °C 23, which was the
conductivity of commercially pure, annealed copper when the standard was set. 24
The Mint used a conductivity meter to test each material as blank planchets in variances of
construction (minimal, nominal, and maximal). Each planchet was tested at two to four
different frequencies. This test is suitable only for non-ferromagnetic materials.

1 siemens (S) is equivalent to the reciprocal of 1 ohm (1/ohm) in the International System of Units; also
referred to as the “mho”; the ohm is a measure of electrical resistance, the siemens is a measure of electrical
conductivity.
23 Equates to 68 °F, or room temperature.
24 Commercially pure, annealed copper at 20 °C today has a higher IACS than 100% because of better methods
for removing impurities from the metal.
22

45

3.3.

Material Tests – Variability Lots

3.3.1. CPZ (Variability Lot)
CPZ failed the wear/durability requirement, and as a result, the Mint eliminated the material

from further consideration.
Progression Strikes

The Mint struck CPZ planchets at strike forces from 33 to 54 tonnes; the detail became
acceptable 25 at 54 tonnes, the same tonnage as the current material, which indicated a
potential for similar die life with this material.
Figure 3-6. CPZ Test Piece

CPZ: 54 tonnes

Steam Test

The color change shown by the CPZ blanks in the variability lot steam test was noticeable,
and was determined to be inferior to the current five-cent material. However, the change
was within acceptable parameters set by the Mint. (The full test results are available in
Appendix 10.2.1.)

“Acceptable” meant sharp, square, level lettering, and fine detail that matched up visually with that in the
dies.

25

46

Figure 3-7. Five-Cent CPZ Blank Color Change—Variability Lot

CPZ’s color changed to a darker hue, with more yellow (higher b) and more red (higher a).

CSV Test

The CSV scans showed acceptable size and EMS measurements for a co-circulate material.
(The full test results are available in Appendix 10.3.1.)
Hardness Test

The Mint tested 48 blank planchets for their hardness, using the Rockwell HR 15T scale.
CPZ showed a hardness range of 66.7 to 70.4, with an average of 68.6. The range of the
samples showed a hardness level slightly higher than that of the current cupronickel.

47

Figure 3-8. Five-Cent CPZ Planchet Hardness Test—Variability Lot

Conductivity

The Mint tested 20 random CPZ blanks each at minimal and nominal plating for their
conductivity. From the lowest to the highest frequencies, CPZ yielded IACS readings of
28.36% to 29.55% and deviations among the pieces tested at each frequency were well
within acceptable parameters.
Copper-Plated Zinc Go/No-Go Determination
Security

Go. CPZ was solely being considered for use in the five-cent, so security needs were
minimal, given the five-cent’s value and the standards in the European Vending Agency
(EVA) Handbook regarding low-denomination coinage. The Mint produced nonsense pieces
and tested them internally and at Coin Acceptor Manufacturers. The material yielded a
unique EMS with respect to other world coins, but it did not match the current material, so
it was considered a co-circulate alternative.
Recyclability

Go. Any condemned or recycled CPZ would be sent directly to the supplier for re-melting
and use in future coin materials. The data suggested this would be relatively cost-neutral,
with the recovered metal’s value offsetting the cost of processing and melting.
Public Health/Toxicity

Go. CPZ presents no unique hazards such as radioactivity or toxicity, and is not a known
allergen. Copper and zinc are used in bathroom and kitchen fixtures as well as current U.S.
coinage (one-cent), so there is significant public exposure and experience with the metals in

48

this material. As such, the Mint was able to state that there are no unique or special hazards
to humans associated with CPZ. 26 Its main hazard would be ingestion/aspiration of the
material, which could cause gastro-intestinal or respiratory issues; this is unrelated to the
material or its use, and so is not a greater or lesser risk for this than any other coin.
Wear Test

No Go. CPZ performed acceptably in one aspect of the wear test, weight loss. During the
two-week test, it lost 3.6mg of its material compared with the 12.9mg lost by the current
material, but the durability of CPZ was insufficient, causing the edges to deform 0.0165”,
more than the 0.010” maximum allowed. Also, the 8µm copper plating was too thin to
withstand the wear, and the high points of the nonsense pieces had worn down to the zinc
substrate, as shown in the photo, below. This was also evident on the pieces subjected to
multiple runs through the CSV to simulate a life of wear in automated CSVs.
Figure 3-9. CPZ After Wear Test

Note the zinc exposure at edges of high points.

As a result of CPZ’s low durability and the weakness of the plating, the Mint determined that
the material failed this test. While plating thickness could be increased to compensate for
the automated coin sorter wear test, the inherent weakness of the zinc substrate when used
for the heavier five-cent (vs. the smaller/lighter one-cent) resulted in the excessive edge
deformation and would not be improved by thicker plating layers. The material supplier has
indicated in technical discussions that there is limited ability to improve the inherent
Dogs and cats that swallow zinc-based coins may be poisoned by the zinc. (Source: CBS News
http://www.cbsnews.com/news/dog-fatally-poisoned-by-one-penny/)
26

49

mechanical properties of the zinc substrate without trading off hardness for ductility. Stated
differently, increasing the hardness and resistance to deformation would significantly impact
the ductility and ability to strike a coin. (The full test results are available in Appendix
10.1.1.)
Co-Circulate

No-Go. CPZ showed a unique EMS, acceptable color change in its steam test, and proved to
have the proper size, weight, edge thickness, and conductivity to co-circulate as a five-cent.
However, CPZ failed the two-week wear test, showing worse edge deformation than the
current material, and the zinc substrate began to show through at the high points on the
design. As a result of this test, CPZ was dropped from consideration and was not evaluated
further.
Go/No-Go Recommendation

No-Go.

50

3.3.2. Tin-Plated Copper-Plated Zinc (Variability Lot)
Tin-plated copper-plated zinc (TPCPZ) failed the wear requirement, and as a result, the Mint
eliminated the material from further consideration.

Progression Strikes

The Mint struck five-cent TPCPZ planchets at strike forces from 50 to 66 tonnes; the detail
became acceptable at 54 tonnes, the same tonnage as the current material, which indicated a
potential for similar die life with this material. Then it struck quarter-dollar planchets at
strike forces from 59 to 67 tonnes; the detail was acceptable at 59 tonnes, well below the
current 62-tonne striking force.
TPCPZ’s dimensional and design fill was superior to the current five-cent and quarter-dollar
materials for the entire range of the progression strikes.
Steam Test

There was almost no color change shown by the TPCPZ blanks in the variability lot steam
test, and the Mint determined TPCPZ to be superior to the current five-cent and quarterdollar materials for this test. As shown in Figures 3-10 and 3-11, below, the “before” and
“after” points are so close, marking them yields no significant data. (The full test results are
available in Appendix 10.2.2.)
Figure 3-10. Five-Cent TPCPZ Blank Color Change—Variability Lot

51

Figure 3-11. Quarter-Dollar TPCPZ Blank Color Change—Variability Lot

CSV Test

The CSV scans showed acceptable size and EMS measurements for a co-circulate material.
(The full test results are available in Appendix 10.3.2.)
Hardness Test

The Mint tested 57 blank five-cent planchets of the for their hardness, using the Rockwell
HR 15T scale. As shown in Figure 3-12, below, TPCPZ showed a hardness range of 65.9 to
68.9, with an average of 67.6. The range of the samples showed a similar hardness level as
the current cupronickel, but slightly harder.
Figure 3-12. Five-Cent TPCPZ Planchet Hardness Test—Variability Lot

52

Next, the Mint tested 55 blank quarter-dollar TPCPZ planchets for their hardness. As shown
in Figure 3-13, below, the quarter-dollar configuration TPCPZ showed a hardness range of
64.2 to 68.0, with an average of 66.9, which was slightly harder than the current material’s
hardness.
Figure 3-13. Quarter-Dollar TPCPZ Planchet Hardness Test—Variability Lot

Conductivity

The Mint tested random five-cent and quarter-dollar TPCPZ blanks at minimum, nominal,
and maximum plating for their conductivity. For the five-cent blanks, from the lowest to the
highest frequencies, TPCPZ yielded IACS readings of 28.50% to 30.71% and deviations
among the pieces tested at each frequency were well within acceptable parameters. The
IACS readings for the quarter-dollar blanks were 28.48% to 30.78% with deviations well
within acceptable parameters.
TPCPZ Go/No-Go Determination
Security

Go. For the five-cent, the security requirements are minimal given its value and the
standards in the EVA Handbook. However, for the quarter-dollar, the security requirements
are more extensive as the coin is near the breakpoint for medium-value coins in the EVA
Handbook. The appropriate level of security for the quarter-dollar was still to be
determined, so the material was rated as “Go” for security.
Test pieces were produced and tested both internally and at Coin Acceptor Manufacturers.
The material yielded a unique EMS with respect to other world coins, but its EMS did not
match the current material so it was considered a co-circulate candidate material.
53

Recyclability

Go. Any condemned or recycled material would go to a brass supplier for re-melting and use
on future brass (non-coin) materials. Zinc and copper are the main constituents in brass
which also has a tin as an additive. The data suggests that this would be relatively costneutral with the recovered metal units offsetting the costs of processing and melting.
Public Health/Toxicity

Go. TPCPZ has no unique hazards such as radioactivity or toxicity, and is not a known
allergen. Tin, copper, and zinc are all commonly used materials and the zinc core with
copper plating is currently used as U.S. coinage (one-cent) and there are no unique or special
hazards to humans associated with it. 27 Its main hazard would be ingestion/aspiration of the
material, which could cause gastro-intestinal or respiratory issues; this is unrelated to the
material or its use, and so is not a greater or lesser risk for this than any other coin.
Wear Test

No Go. After only two days in the tumbler, the tin plating and copper plating on the TPCPZ
pieces had worn almost completely away from the zinc substrate, as shown in the picture,
below. The Mint conducted a second round of wear testing, which confirmed the earlier
failure. The material failed this test. (The full test results are available in Appendix 10.1.2.)
Figure 3-14. TPCPZ After Wear Test

Note the fragments of plating remaining around the edge of the piece.

27

Dogs and cats that swallow coins with a zinc core may be poisoned by the zinc. (Source: CBS News.)

54

Co-Circulate

No-Go. TPCPZ showed a unique EMS, acceptable color change in its steam test, and proved
to have the proper size, weight, edge thickness, and conductivity to co-circulate.
Unfortunately, it failed the two-week wear test, with the plating wearing away nearly
completely in only two days. As a result of this test, TPCPZ was dropped from consideration
and was not tested further in the pre-production lots.
Go/No-Go Recommendation

No-Go.

55

3.3.3. Multi-Ply-Plated Steel (Variability Lot)
Multi-Ply-Plated Steel (MPPS) passed all of its Go/No-Go criteria for both the five-cent and
the quarter-dollar, except security levels needed for the quarter-dollar were still being
evaluated. Testing continued through the pre-production lots for this material at that
denomination. As its EMS signature and weight differ significantly from the current coins,
MPPS is considered a co-circulation option.
Progression Strikes

The Mint struck five-cent and quarter-dollar MPPS planchets at strike forces from 30 to 60
tonnes. The current five-cent tonnage is 54 tonnes; at 54 and 60 tonnes, MPPS fill was poor.
The Mint observed abrasive wear scratches in the progression strikes, attributed to the
abrasive nature of the pure-nickel surface coating. For any extensive striking such as preproduction lots, PVD-coated dies 28 would be required.
Figure 3-14. MPPS Five-Cent Test Piece

Red arrows indicate areas of poor fill.

Physical vapor deposition is a vacuum deposition method involving plasma sputter bombardment of target
material to deposit thin films of that material onto surfaces (i.e., coining dies). PVD coatings are generally used
to improve hardness and wear resistance. The RCM routinely uses this coating process on their numismatic and
circulating dies; for further testing, the Mint sent dies to the RCM for PVD coating.
28

56

The current quarter-dollar tonnage is 62 tonnes, but the MPPS quarter-dollar nonsense
pieces needed 65 tonnes to see acceptable fill in the lettering along the edge.
Figure 3-15. MPPS Quarter-Dollar Test Piece

Steam Test

There was almost no color change shown by the MPPS blanks in the variability lot steam
test, and the Mint determined MPPS to be superior to the current five-cent and quarterdollar materials for this test. As shown in Figures 3-16 and 3-17, below, the “before” and
“after” points are so close, marking them yields no significant data. (The full test results are
available in Appendix 10.2.4.)
Figure 3-16. Five-Cent MPPS Blank Color Change—Variability Lot

57

Figure 3-17. Quarter-Dollar MPPS Blank Color Change—Variability Lot

CSV Test

The CSV scans showed acceptable size and EMS measurements for a co-circulate material.
(The full test results are available in Appendix 10.3.4.)
Hardness Test

The Mint tested 29 blank MPPS five-cent planchets for their hardness, using the Rockwell
HR 15T scale. As shown in Figure 3-18, below, MPPS showed a hardness range of 64.3 to
69.7, with an average of 68.1. The range of the samples showed a similar hardness level as
the current cupronickel, but slightly harder.
Figure 3-18. Five-Cent MPPS Planchet Hardness Test—Variability Lot

58

Next, the Mint tested 27 blank quarter-dollar MPPS planchets for their hardness. As shown
in Figure 3-19, below, MPPS showed a hardness range of 63.8 to 67.4, with an average of
65.3, which was almost identical to the current material’s hardness.
Figure 3-19. Quarter-Dollar MPPS Planchet Hardness Test—Variability Lot

Conductivity

The conductivity test is appropriate for measuring non-ferromagnetic metals and alloys. The
construction of the MPPS planchet makes this test not applicable due to the combination of
non-ferromagnetic plating and ferromagnetic steel substrate, so it was not performed.
Conductivity was measured in the CSV test (see above), which uses sensors capable of
measuring the relative electromagnetic properties of both ferromagnetic and nonferromagnetic metals.
MPPS Go/No-Go Determination
Security

Go. For the five-cent, the security requirements are minimal given its value and the
standards in the EVA Handbook. At the time of variability testing, no security
determination had been established for the quarter-dollar, so the material was approved for
pre-production testing.
Nonsense pieces were tested both internally and at coin acceptor manufacturers. MPPS
exhibits a distinguishable EMS, but has a broader conductivity band that can overlap with
other world coins. The steel core also makes MPPS more easily counterfeited, which has a
greater potential impact on the quarter-dollar, as it is more widely used in vending.

59

Recyclability

Go. Any condemned or recycled material would go to a stainless steel supplier for remelting and use on other non-coin materials. The data suggests that this would be relatively
cost-neutral with the recovered metal units offsetting the cost of processing and melting.
However, with the presence of copper, the ability to absorb large quantities of MPPS as
stainless scrap is limited and may impact the recyclability of the larger quantities that would
be generated if the material was used for U.S. coinage. The Mint contacted two domestic
stainless steel mills that reported that the percentage of stainless material containing copper
was 40 percent of one supplier’s volume and only 15 percent of the other’s. Depending on
the volume and timing, then, recycling could be limited.
Public Health/Toxicity

Go. MPPS has no unique hazards such as radioactivity or toxicity, and is not a significant
allergen. It is a material used in a number of applications worldwide, including coinage.
There are no unique or special hazards associated with it. The nickel coating can cause skin
rashes in some small portion of the population with an occurrence possibly higher than the
current five-cent or quarter-dollar material which has been acceptable. Its main hazard
would be ingestion/aspiration of the material, which could cause gastro-intestinal or
respiratory issues; this is unrelated to the material or its use, and so is not a greater or lesser
risk for this than any other coin.
Wear Test

Go. MPPS performed exceptionally well in the two-week wear test, as the five-cent
nonsense pieces lost an average of 14.1mg of the material compared with the 19.0mg lost by
the current material. The quarter-dollar nonsense pieces performed even better, losing only
an average of 4.4mg compared with the 27.2mg lost by the current material. In the five-cent
configuration, MPPS’ edge deformation was less than the current material, and in the
quarter-dollar configuration, MPPS deformed only 0.005” more than the current material,
well within the 0.01” allowed. (The full test results are available in Appendix 10.1.4.)

60

Figure 3-20. MPPS Quarter-Dollar After Wear Test

Co-Circulate

Go. MPPS showed acceptable color change in its steam test, and proved to have the proper
size, weight, edge thickness, and conductivity to co-circulate. It also showed a superior
resistance to wear, but needed more tonnage to strike and caused wear to the dies. The Mint
determined that this likely could be mitigated with further testing. Security for the quarterdollar was still being determined, so the team considered MPPS a valid candidate for cocirculation in pre-production testing for both the five-cent and the quarter-dollar.
Go/No-Go Recommendation

Go.

61

3.3.4. Nickel-Plated Steel (Variability Lot)
Nickel-Plated Steel (NPS) passed all of its Go/No-Go criteria for both the five-cent and the
quarter-dollar, except the Mint was still evaluating the security levels needed for the

quarter-dollar. Testing continued through the pre-production lots for this denomination. As
its EMS signature and weight differ significantly from the current coins, NPS is considered a
co-circulation option.
Progression Strikes

The Mint struck five-cent NPS planchets at strike forces from 30 to 65 tonnes. The current
five-cent tonnage is 54 tonnes, and at this tonnage, NPS fill matched the current material’s,
but edge thickness was insufficient until 58 tonnes. Abrasive wear scratches in the
progression strikes were attributed to the abrasive nature of the pure-nickel surface layer.
For any extensive striking such as pre-production runs, PVD-coated dies would be required.
Figure 3-21. NPS Five-Cent Test Piece

Red arrows indicate abrasive wear scratches

62

The Mint then struck quarter-dollar planchets at strike forces from 36 to 73 tonnes. NPS fill
and coin diameter were unacceptable across the entire range of progression strikes.
Figure 3-22. NPS Quarter-Dollar Test Piece

Red areas indicate insufficient fill.

Steam Test

The NPS blanks showed a slight color change in the variability lot steam test, making the
blanks darker, but the change was small. The Mint determined NPS to be superior to the
current five-cent and quarter-dollar materials for this test. As shown in Figures 3-23 and
3-24, below, the five-cent and quarter-dollar saw nearly identical color changes, with
the hue going slightly more yellow and more red. (The full test results are available in
Appendix 10.2.3.)
Figure 3-23. Five-Cent NPS Blank Color Change—Variability Lot

63

Figure 3-24. Quarter-Dollar NPS Blank Color Change—Variability Lot

CSV Test

The CSV scans showed acceptable size and EMS measurements for consideration as a cocirculate material. (The full test results are available in Appendix 10.3.3.)
Hardness Test

The Mint tested 65 blank NPS five-cent planchets for their hardness, using the Rockwell HR
15T scale. As shown in Figure 3-25, below, NPS showed a hardness range of 76.4 to 78.9,
with an average of 77.3, well above the upper limit for the current cupronickel.
Figure 3-25. Five-Cent NPS Planchet Hardness Test—Variability Lot

Next, the Mint tested 57 blank NPS quarter-dollar planchets for their hardness. As shown in
Figure 3-26, below, NPS showed a hardness range of 74.4 to 79.4, with an average of 77.4.
The range of the samples showed a similar hardness level to the five-cent pieces, well above
the upper limit for the current cupronickel.
64

Figure 3-26. Quarter-Dollar NPS Planchet Hardness Test—Variability Lot

Conductivity

The conductivity test is appropriate for measuring non-ferromagnetic metals and alloys. The
construction of the NPS planchet makes this test not applicable due to the combination of
non-ferromagnetic plating and ferromagnetic steel substrate, so it was not performed.
Conductivity was measured in the CSV test (see above), which uses sensors capable of
measuring the relative electromagnetic properties of both ferromagnetic and nonferromagnetic metals.
NPS Go/No-Go Determination
Security

Go. For the five-cent, the security requirements are minimal given its value and the
standards in the EVA Handbook. However, for the quarter-dollar, the security requirements
are more extensive as the coin is near the breakpoint for medium-value coins in the EVA
Handbook. At the time of variability testing, no security determination had been established
for the quarter-dollar, so the material was approved for pre-production testing.
Recyclability

Go. The recycle path for any condemned or recycled material would be directly to a
stainless steel supplier for re-melting and for use on other, non-coin materials. The data
suggests that this would be relatively cost-neutral with the recovered metal units offsetting
the costs of processing and melting. As iron (steel) and nickel are both present in all stainless
steel grades, there would not be any limitation on accepting the scrap for remelting.

65

Public Health/Toxicity

Go. NPS has no unique hazards such as radioactivity or toxicity, and is not a significant
allergen. It is a material used in a number of applications worldwide, including coinage.
There are no unique or special hazards associated with it. The nickel coating can cause skin
rashes in some small portion of the population with an occurrence possibly higher than the
current five-cent or quarter-dollar material which has been acceptable. Its main hazard
would be ingestion/aspiration of the material, which could cause gastro-intestinal or
respiratory issues; this is unrelated to the material or its use, and so is not a greater or lesser
risk for this than any other coin.
Wear Test

Go. NPS performed supremely well in the two-week wear test, as the five-cent nonsense
pieces lost an average of 7.7mg of the material compared with the 24.5mg lost by the current
material. The quarter-dollar nonsense pieces performed equally well, losing only an average
of 5.8mg compared with the 27.2mg lost by the current material. In the five-cent
configuration, NPS’ edge deformation was less than the current material; in the quarterdollar configuration, NPS’ edge deformation was identical to the current material. (The full
test results are available in Appendix 10.1.3.)
Figure 3-27. NPS Quarter-Dollar After Wear Test

NPS quarter-dollar nonsense piece after wear test

Co-Circulate

Go. NPS showed acceptable color change in its steam test, and proved to have the proper
size, weight, edge thickness, and conductivity to co-circulate. It also showed a superior
resistance to wear, but needed more tonnage to strike and caused wear to the dies. The Mint
determined that this could be mitigated with further testing. Security for the quarter-dollar
66

was still being determined, so the team considered NPS a valid candidate for co-circulation
in pre-production testing for both the five-cent and the quarter-dollar.
Go/No-Go Recommendation

Go.

67

3.3.5. Cupronickel 80/20 from Supplier A (80/20A) (Variability Lot)
Cupronickel 80/20 from Supplier A (80/20A) passed all of its Go/No-Go criteria for the fivecent except for the EMS test. 80/20A was intended to be a seamless alternative, but its EMS

was too far out of the current material’s range. The Mint pursued an alternative composition
for 80/20 from Supplier B (see 3.3.6), and 80/20A was deferred from further testing during
Phase II to allow the Mint to focus on refining the B composition, which was closer to the
current material’s EMS.
Progression Strikes

Due to a limited number of blanks available for testing, the Mint did not conduct progression
strikes for 80/20A. Instead, the Mint struck five-cent planchets at the current five-cent
tonnage of 54 tonnes. At this tonnage, 80/20A achieved acceptable design and dimensional
fill that was similar to those of the current five-cent. The Mint observed no difficult-to-fill
areas.
Figure 3-28. 80/20A Test Piece (54T Strike)

Steam Test

The 80/20A blanks showed random, large, water stains in the variability lot steam test,
making the blanks’ test results exceedingly variable and rendering the test inconclusive.
(The full test results are available in Appendix 10.2.5.)
CSV Test

The CSV scans showed acceptable size measurements but unacceptable EMS results for
consideration as a seamless material. (The full test results are available in Appendix 10.3.5.)
Hardness Test

The Mint tested 31 blank 80/20A five-cent planchets for their hardness, using the Rockwell
HR 15T scale. As shown in Figure 3-29, below, 80/20A showed a hardness range of 61.6 to
68

64.2, with an average of 63.0. The range of the samples showed a hardness level well within
the range of the current cupronickel but slightly softer on average. For cupronickel, the
hardness was not a function of just the composition, but also the annealing. These pieces
were subject to a laboratory anneal which contributed to the lower hardness observed.
Figure 3-29. Five-Cent 80/20A Planchet Hardness Test—Variability Lot

Conductivity

The Mint tested six batches of five random 80/20A blanks each at minimal and nominal
composition for their conductivity. From the lowest to the highest frequencies, 80/20A
yielded IACS readings of 5.61% to 6.93% and deviations among the pieces tested at each
frequency were well within acceptable parameters.
80/20A Go/No-Go Determination
Security

Go. For the five-cent, the security requirements are minimal given its value and the
standards in the EVA Handbook. 80/20A proved to have the same level of security as the
current material, with a unique EMS, an uncommon alloy, and no use in other mints.
Recyclability

Go. The recycle path for any condemned or recycled material would be directly to the coin
material supplier for re-melting and for use on coin materials. The data suggests that this
would be cost-positive with the recovered metal units more than offsetting the costs of
processing and melting.

69

Public Health/Toxicity

Go. As a cupronickel alloy, there are no unique hazards such as radioactivity or toxicity, and
it is not a significant allergen. The nickel content can be a cause for skin rashes in some
small portions of the population with an occurrence similar to the current five-cent material.
Its main hazard would be ingestion/aspiration of the material, which could cause gastrointestinal or respiratory issues; this is unrelated to the material or its use, and so is not a
greater or lesser risk for this than any other coin.
Wear Test

Go. 80/20A performed well in the two-week wear test, as the five-cent nonsense pieces lost
an average of 19.5mg of the material compared with the 20.3mg lost by the current material.
Edge deformation in the five-cent configuration was only 0.005” more than the current
cupronickel, half of the 0.010” allowable deformation. (The full test results are available in
Appendix 10.1.5.)
Figure 3-30. 80/20A After Wear Test

Seamless

No-Go. 80/20A showed staining in its steam test, but proved to have the proper size, weight,
edge thickness, and conductivity for a seamless candidate. It also showed good resistance to
wear, and comparable strike tonnage. Its EMS, however, was too far out of the acceptable
range for a seamless candidate. The team therefore deferred 80/20A as a candidate.
Go/No-Go Recommendation

No-Go.

70

3.3.6. Cupronickel 80/20 from Supplier B (80/20B) (Variability Lot)
Cupronickel 80/20 from Supplier B (80/20B) passed all of its Go/No-Go criteria for the five-

cent as a seamless alternative. The Mint requested this material as a development step in

conjunction with the 80/20A, and had the supplier change the material to 77% Cu/19.7%
Ni/3.3% Mn, which showed a promising EMS match.
Progression Strikes

Due to a limited number of blanks available for testing, the Mint did not conduct progression
strikes for 80/20B. Instead, the Mint struck five-cent planchets at the current five-cent
tonnage of 54 tonnes. At this tonnage, 80/20B achieved acceptable design and dimensional
fill that was similar to those of the current five-cent. The Mint observed no difficult-to-fill
areas.
Figure 3-31. 80/20B Test Piece (54T Strike)

Steam Test

The 80/20B blanks showed random, large, water stains in the variability lot steam test,
making the blanks’ test results exceedingly variable and rendering the test inconclusive.
(The full test results are available in Appendix 10.2.6.)
CSV Test

The CSV scans showed acceptable size measurements and acceptable EMS results for
consideration as a potentially seamless material with minor adjustments to the composition.
(The full test results are available in Appendix 10.3.6.)
Hardness Test

The Mint tested 33 blank 80/20B five-cent planchets for their hardness, using the Rockwell
HR 15T scale. As shown in Figure 3-32, below, 80/20B showed a hardness range of 67.4 to
70.0, with an average of 68.7. The range of the samples showed a hardness level well within
71

the range of the current cupronickel but slightly harder on average. Whether this was
related to composition changes, use of a laboratory anneal or both could not be determined.
Figure 3-32. Five-Cent 80/20B Planchet Hardness Test—Variability Lot

Conductivity

The Mint tested three batches of 25 random 80/20B blanks each at minimal and nominal
composition for their conductivity. From the lowest to the highest frequencies, 80/20B
yielded IACS readings of 5.00% to 5.99% and deviations among the pieces tested at each
frequency were well within acceptable parameters.
80/20B Go/No-Go Determination
Security

Go. For the five-cent, the security requirements are minimal given its value and the
standards in the EVA Handbook. 80/20B proved to have the same level of security as the
current material, with a unique EMS, an uncommon alloy, and no use in other mints.
Recyclability

Go. Any condemned or recycled material would go directly to the coin material supplier for
re-melting and for use on coin materials. The data suggests that this would be cost positive
with the recovered metal units more than offsetting the costs of processing and melting.
Public Health/Toxicity

Go. As a cupronickel alloy, there are no unique hazards such as radioactivity or toxicity, and
it is not a significant allergen. The nickel content can be a cause for skin rashes in some
small portions of the population with an occurrence similar to the current five-cent material,
which has been acceptable. Its main hazard would be ingestion/aspiration of the material,
72

which could cause gastro-intestinal or respiratory issues; this is unrelated to the material or
its use, and so is not a greater or lesser risk for this than any other coin.
Wear Test

Go. 80/20B performed well in the two-week wear test, as the five-cent nonsense pieces lost
an average of 16.8mg of their material compared with the average of 19mg that the current
pieces lost. Edge deformation in the five-cent configuration was measured at the 0.010”
allowable deformation. (The full test results are available in Appendix 10.1.6.)
Figure 3-33. 80/20B After Wear Test

Seamless

Go. 80/20B showed staining in its steam test, but proved to have the proper size, weight,
edge thickness, and conductivity for a potentially seamless candidate. It also showed good
resistance to wear, and comparable strike tonnage. The material has an EMS that can be read
by vending machines and other coin handling equipment. Its signature is very similar to that
of the current material and could potentially be seamless with further composition changes.
Go/No-Go Recommendation

Go.

73

3.4.

Pre-Production Testing

The materials that passed Go/No-Go—nickel-plated steel, multi-ply-plated steel, and
80/20B—were subjected to many of the same tests in pre-production as they saw in
variability. The materials were purchased in their standard configurations (not purchased in
minimum, maximum, and nominal variances) expected to be seen in normal production.
Die life and die wear were not tested in variability lots, but both were considerations in preproduction testing. Other tests that had been performed in variability lots (wear, steam color
change, CSV) were applied to the pre-production lots to determine how well the materials
performed at their standard configurations.
Materials in pre-production testing were put through a down-selection process at the end of
testing, in which they each were measured against current coinage materials to determine
their feasibility for use in U.S. coinage.
Both nickel-plated steel and multi-ply-plated steel were tested in five-cent and quarterdollar configurations while 80/20B was tested only in the five-cent configuration (with the
understanding that it could replace the current clad material in the dime, quarter-dollar, and
half-dollar if it passed as a seamless alternative for the cupronickel five-cent).
3.4.1. CPZ Pre-Production Data
The Mint purchased CPZ for pre-production and the pre-production tests were completed

before the Mint had finalized the optimization of the wear test. Therefore, when CPZ failed
its Go/No-Go determination (due to durability of plating thickness and substrate), even
though the Mint had already run the pre-production tests, CPZ was not put through a downselection process. (CPZ’s pre-production test data is included in this report only as reference
through Appendix 10.4.)
3.4.2. Down-Selection Matrices
The following tables summarize the down-selection process for the co-circulate materials

that passed Go/No-Go. In all cases, criteria were rated in two tiers: Comparable or Better,
and Less than Current.

74

Multi-Ply-Plated Steel (Five-Cent)

75

Nickel-Plated Steel (Five-Cent)

76

Stainless Steel (Five-Cent)

77

Multi-Ply-Plated Steel (Quarter-Dollar)

78

Nickel-Plated Steel (Quarter-Dollar)

79

3.4.3. Multi-Ply-Plated Steel (Pre-Production Lot)
For pre-production testing, the upset profiles of the Multi-Ply-Plated Steel (MPPS) planchets

were modified from those used in variability lots. MPPS passed its down-selection criteria
for the five-cent, with Comparable or Better in half of its criteria, but it rated Less than
Current in four of the six criteria for the quarter-dollar, including for coinability and

counterfeit/slug vulnerability. MPPS showed insufficient fill in both five-cent and quarterdollar denominations in the progression strikes, only seeing complete fill above the current
strike force, and seeing a significantly greater rate of die failure than seen with the current
material.
The RCM PVD-coated the dies for pre-production testing, and the coating worked to
prevent abrasive wear when striking the nickel surface of the planchets. Polishing the dies
before PVD coating extended the die life, but the dies still failed in under 250,000 strikes
(less than half the baseline of 500,000 strikes).
Progression Strikes

The Mint struck five-cent MPPS planchets at strike forces from 20 to 60 tonnes. The current
five-cent tonnage is 54 tonnes, and at this and 56 tonnes, MPPS fill was poor. The PVD
coating on the dies succeeded in preventing abrasive wear scratches from appearing in struck
pieces.
Figure 3-34. MPPS Five-Cent Test Piece (56T Strike)

The top of Martha’s bonnet, near the upper-left edge, shows insufficient fill

80

The Mint struck quarter-dollar MPPS planchets at strike forces from 36 to 64 tonnes. The
current quarter-dollar tonnage is 62 tonnes; design/border fill was acceptable at 55 tonnes,
but the MPPS nonsense pieces needed 64 tonnes to see acceptable fill in the lettering along
the edge. The early fill at the border likely “locked” the metal at the border of the planchets,
preventing the material in the center of the planchet from flowing out to the border and
filling in the letters in the die. This necessitated the increase in strike force that may have
contributed to die failure.
Figure 3-35. MPPS Quarter-Dollar Test Piece (64T Strike)

The Mint determined that five-cent and quarter-dollar MPPS pieces struck with polished,
PVD-coated dies performed worse than with the current material in terms of strike force and
die life.
The Mint also observed a greater rate of crack/piece-out incidents and a higher die-lifefailure rate than the current material, seeing die pairs last an average of 200,000 strikes
before they had to be replaced (as compared to the nominal 500,000). Two sets of
unpolished, PVD-coated dies saw cracks form at just over 20,000 strikes, illustrating that
polishing of the die would be necessary.
Further research will be needed to determine what the optimized die life will be, but it is
anticipated to be fewer than 500,000 strikes. RCM’s current average die life, after years of
producing MPPS coins, is 350,000 strikes. A financial analysis can be done on how the loss
in productivity impacts the anticipated material cost savings.

81

Steam Test

There was little color change shown by the MPPS blanks in the pre-production lot steam
test, and the Mint determined MPPS to be superior to the current five-cent and quarterdollar materials for this test. The results are shown in Figures 3-36 and 3-37, below, with the
“before” point lower and to the left of the “after” point in each graph. (The full test results
are available in Appendix 10.5.2.)
Figure 3-36. Five-Cent MPPS Blank Color Change—Pre-Production Lot

Figure 3-37. Quarter-Dollar MPPS Blank Color Change—Pre-Production Lot

82

CSV

The CSV tests showed acceptable conductivity, size, and EMS measurements for a cocirculate material, though the EMS was not unique among world coins, contributing to a
security concern about the application of this material to the quarter-dollar. (The full test
results are available in Appendix 10.6.2, at the end of this report.)
Hardness Test

The Mint tested two lots of 255 blank MPPS five-cent planchets and two lots of 255 blank
MPPS quarter-dollar planchets for their hardness, using the Rockwell HR 15T scale. MPPS
showed a hardness range of 65.4 to 69.9 with an average of 67.9 in the five-cent, and a range
of 65.3 to 73.6 with an average of 68.8 in the quarter-dollar, almost identical to the hardness
shown in the variability lots. The range of the samples showed a slightly harder level than
the current cupronickel.
Wear Test

MPPS performed even better in the two-week wear test for pre-production than it had in
variability. The five-cent and quarter-dollar nonsense pieces both lost an average of 3.4mg of
the material compared with the 19.0mg lost by the current five-cent material and the 27.2mg
lost by the current quarter-dollar material. Edge deformation in the five-cent and quarterdollar MPPS was less than the deformation shown by the current material. (The full test
results are available in Appendix 10.4.2.)
3.4.4. MPPS Down-Selection

Environmental Impact

Comparable or Better. As MPPS is a plated material being tested as a replacement for the
monolithic five-cent and the three clad denominations, data suggests that the use of this
material would have a negative impact on the waste stream. However, this impact could be
effectively mitigated.
Supply Chain

Less than Current. All the raw materials in MPPS are in adequate supply, but the Royal
Canadian Mint has a pending U.S. patent extension application on this material, effectively
reducing the number of established suppliers to one, as compared to the current two
suppliers for both the five-cent and the quarter-dollar.
Coinability

Less than Current. Pre-production strikes of standard-crown dies at comparable tonnage to
the current strike force saw a significantly greater rate of failure to the dies than seen with
83

current materials. The Mint also observed inferior fill rates at comparable tonnage to the
current material. More testing will be needed to see if these issues can be mitigated.
Recyclability

Less than Current. MPPS sees an inferior recycling option compared with current materials.
While steel and nickel are both sought by stainless steel manufacturers, the inclusion of
copper in this material limits its scrap market. Copper-bearing stainless steel grades made up
only 40 percent and 15 percent at two domestic stainless steel plants, illustrating the
limitations presented by the copper plating. The material is recyclable, for non-coin use
only, but there is a potential land-fill issue with the volume of coins the Mint would likely
recycle (based on the number of coins currently sent back to suppliers by the Mint).
Durability

Comparable or Better. The Mint observed a superior wear rate after the wear test and
minimal discoloration after the steam test with MPPS. MPPS showed a wear rate 82 percent
lower than the current material.
Counterfeit/Slug Vulnerability (Quarter-Dollar Only)

Less than Current. MPPS has a ferromagnetic core made of a very common material. The
plating of this material is easily replicated and easily counterfeited (in testing, a steel slug
plated for a few minutes in a copper solution (using only a battery) and another steel slug
with aluminum foil taped to it were both accepted by two different coin acceptors as MPPS
quarter-dollars). MPPS’ EMS was also found to vary far more than the current quarter-dollar
and was not unique among world coins. (The Philippine one-peso coin, for example, is
approximately the same size as the quarter-dollar and is made of MPPS, but is only worth
about $0.02.) The Mint determined that MPPS’ security was lesser than the current quarterdollar’s.
Feasibility

Five-Cent – Feasible
Quarter-Dollar – Not Feasible

84

3.4.5. Nickel-Plated Steel (Pre-Production Lot)
Nickel-Plated Steel (NPS) rated as Comparable or Better for half of its Down Selection

criteria as a co-circulate option for the five-cent and the quarter-dollar, but it rated as Less
than Current in coinability, recyclability, and counterfeit/slug vulnerability (which did not
apply to the five-cent).
After the variability testing was complete, the Mint provided feedback to The Royal Mint
(RM) technical representatives and subsequently RM revised the upset profiles and sent
small quantities of planchets (five-cent and quarter-dollar) called “Pilot lots.” The RM also
PVD-coated the dies to alleviate the abrasion of the blanks’ nickel surface, but the Mint still
observed a significantly greater rate of die failure than seen with the current material. Some
die pairs were polished before PVD coating and others were not, to determine what
difference, if any, polishing would make.
The Mint conducted further progression strikes, and quarter-dollar progression strikes
demonstrated improvements from the previous strike, but required 66 tonnes to achieve
acceptable design fill and coin dimensions. The border achieved fill at only 58 tonnes, which
likely “locked” the metal at the border of the planchets, preventing the material in the center
of the planchet from flowing out to the border and filling in the detail in the die.
Figure 3-38. NPS Quarter-Dollar Test Piece (66T Strike)

Revised-upset five-cent planchets produced test pieces with worse design fill and coin edge
thickness than those of the previous progression strikes. Again, feedback was provided to
RM for improvement to the five-cent upset profile prior to receiving pre-production
quantities. Changes were also requested for the quarter-dollar to counter the die-failure rate.

85

The revised-upset quarter-dollar NPS planchets arrived in late July. In spite of the changes
requested for the quarter-dollar planchets, design fill and coin edge thickness were still
worse than those of the previous progression strikes. Die-life failure rates were also
drastically higher with this material than with the current material. The data suggests that
this material will continue to have issues with strike force and die-life failure regardless of
changes made to the coining system.
Figure 3-39. NPS Five-Cent Test Piece (Detail)

NPS five-cent: edge lettering showing poor letter fill

Progression Strikes

After receiving the pre-production lots, the Mint struck five-cent NPS planchets at strike
forces from 20 to 60 tonnes. The current five-cent tonnage is 54 tonnes, and at this and 56
tonnes, NPS fill was acceptable. The PVD coating on the dies succeeded in preventing
abrasive wear scratches from appearing in struck pieces.
The Mint struck quarter-dollar NPS planchets at strike forces from 36 to 64 tonnes. The
current quarter-dollar tonnage is 62 tonnes; design/border fill was acceptable at 55 tonnes,
but the NPS nonsense pieces needed 64 tonnes to see acceptable fill in the lettering along the
edge.
The rates of die failure with NPS were greater than that seen with the current material, as
PVD-coated die pairs failed on an average of 261,000 strikes, below the baseline level of the
current material and standard dies, which was 500,000. Dies that were not polished before
PVD coating failed on an average of 77,000 strikes. Cracks presented on both the obverse
(bonnet area) and reverse (building top corner to coin edge) of the dies.

86

The Mint determined the coating failures were related to metal oxides on the dies’ surfaces.
PVD coatings typically do not adhere as well to metal oxides as they do to elemental metal.
The RM dies were relatively free of surface oxides after heat treatment and their follow-on
polishing operation removed what thin oxide layer may have been present. U.S. Mint dies
have much thicker oxide layers and limited post-finishing operation to remove these layers.
The significant difference in die life seen between the non-polished and polished dies
indicated that future dies would need to be polished to provide a more-uniform surface and
one that was free of oxides.
The five-cent planchets and struck pieces further exhibited indications of poor lubrication, a
condition that needs to be investigated further. The team saw unacceptable, excessive wear
on the press parts, especially the press’s mechanical “fingers” that move the planchets into
position at the dies and the conveyor belts that take struck coins away. The excessive wear
must be resolved to support sustained coining operations.
Improved coinability and die life could be achieved with an optimization of the die designs
to be more compatible with the NPS material. The hardness check on the retained planchets
showed NPS to be approximately 20 percent harder than the current material. Also, the
upset profile of the planchets appeared sharper than the current material’s flatter
configuration. Both of these, along with the poor lubrication, could also have contributed to
the excessive equipment wear.
While it is possible to double the die life with changes in coin features and lubrication, it is
not likely that these changes alone will improve the die-life gap. Some reduction in die life
is to be expected with this alternative material. The die life achieved by RM is around
600,000 strikes for the 5-pence and 10-pence coins. Other countries that RM has supplied
with NPS have an average of 447,000 strikes with a range from 215,000 to 800,000. This
average is on coins with differing features, and the quality standards for those mints are
unknown. Given the need for coin changes and the lower anticipated die life, this material is
considered as Less than Current for coinability and die wear.
Further research will be needed to determine what the optimized die life will be, but it is
anticipated to be less than 500,000 strikes. A financial analysis can be performed on how the
loss in productivity impacts the anticipated material cost savings.

87

Steam Test

There was little color change shown by the NPS blanks in the pre-production lot steam test,
and the Mint determined NPS to be superior to the current five-cent and quarter-dollar
materials for this test. The results are shown in Figures 3-40 and 3-41, below, with the
“before” point lower and to the left of the “after” point in each graph. (The full test results
are available in Appendix 10.5.1.)
Figure 3-40. Five-Cent NPS Blank Color Change—Pre-Production Lot

Figure 3-41. Quarter-Dollar NPS Blank Color Change—Pre-Production Lot

88

CSV

The CSV tests showed acceptable conductivity, size, and EMS measurements for a cocirculate material, though the EMS was not unique among world coins, contributing to this
material’s security failure for the quarter-dollar. (The full test results are available in
Appendix 10.6.1.)
Hardness Test

The Mint tested two lots of 255 blank NPS five-cent planchets and two lots of 255 blank NPS
quarter-dollar planchets for their hardness, using the Rockwell HR 15T scale. NPS showed a
hardness range of 65.4 to 69.9 with an average of 67.9 in the five-cent, and a range of 65.3 to
73.6 with an average of 68.8 in the quarter-dollar, almost identical to the hardness seen in
the variability lots. The range of the samples showed a higher hardness level than the
current cupronickel.
Wear Test

As in the variability lot wear test, NPS performed exceptionally well, with a wear rate
72 percent lower than the current material (4.6mg v. 19mg for five-cent and 7.5mg v. 27.2mg
for the quarter-dollar). In addition, the five-cent and the quarter-dollar NPS pieces showed
an average edge deformation lower than that shown by the current material. (The full test
results are available in Appendix 10.4.1.)
3.4.6. NPS Down-Selection

Environmental Impact

Comparable or Better. As NPS is a plated material being tested as a replacement for the
monolithic five-cent and the three clad denominations, the data suggests that the use of NPS
would have a negative impact on the waste stream. However, that impact could be
effectively mitigated.
Supply Chain

Comparable or Better. All the raw materials in NPS are in adequate supply. There are at
least two established suppliers, which is identical to the current two suppliers for both the
five-cent and the quarter-dollar.
Coinability

Less than Current. Pre-production strikes of standard-crown dies at comparable tonnage to
the current material had a significantly greater rate of die failure than with current materials.
The Mint also observed that changes The Royal Mint made to the upset profile between the
Pilot lot and the pre-production lot improved the fill on progression strikes dramatically.
89

The Mint also saw more wear on the press machinery, from the feed bowl, the mechanical
“fingers” that move planchets into the press, and the conveyor belt that carries the new coins
away. In some of these cases, parts that normally would last weeks required changing every
eight hours or less.
Recyclability

Less than Current. NPS sees an inferior recycling option compared with current materials.
While steel and nickel are both sought by stainless steel manufacturers, the recyclability
would be for non-coin use only.
Durability

Comparable or Better. The Mint observed a superior wear rate and minimal discoloration
with NPS. NPS showed a wear rate of only 18 percent, below the maximum 20 percent set
by the Mint.
Counterfeit/Slug Vulnerability (Quarter-Dollar Only)

Lesser than Current. NPS has a ferromagnetic core and is made of commonly used, readily
available materials. NPS’ plating is easily replicated (many web sites have simple instructions
on how to nickel-plate objects such as coins). The EMS was wider than the current quarterdollar and was not unique among world coins. (The Nigerian 50-Kobo coin, for example, is
approximately the same size as the quarter-dollar and is made of NPS, but is only worth
$0.003.) The Mint determined that NPS’ security was lesser than the current quarter-dollar’s.
Feasibility

Five-Cent – Feasible
Quarter-Dollar – Not Feasible

90

3.4.7. Cupronickel 80/20B (Pre-Production Lot)
Cupronickel 80/20 supplied by Supplier B (80/20B) rated as Comparable or Better for all of its

Down Selection criteria as a seamless option for the five-cent, and is expected to perform
equally well as cladding for the dime, quarter-dollar, and half-dollar (testing to begin in
Phase III).
Progression Strikes

The Mint struck five-cent 80/20B planchets at strike forces from 20 to 60 tonnes. The
current five-cent tonnage is 54 tonnes, and at this and 56 tonnes, 80/20B fill was acceptable.
Figure 3-44. 80/20B Test Piece (54T Strike)

Steam Test

There was little color change shown by the 80/20B blanks in the pre-production lot steam
test, and the Mint determined 80/20B to be comparable to the current five-cent material for
this test. The results are shown in Figure 3-43, below, with the “before” point lower and to
the left of the “after” point in the graph. (The full test results are available in Appendix
10.5.3.)

91

Figure 3-45. Five-Cent 80/20Blank Color Change—Pre-Production Lot

CSV

The CSV tests showed acceptable size measurements for a seamless material, and an EMS that
matched the current five-cent. (The full test results are available in Appendix 10.6.3.)
Hardness Test

The Mint tested two lots of 255 blank 80/20B five-cent planchets, using the Rockwell HR
15T scale. 80/20B showed a hardness range of 65.4 to 69.9 with an average of 67.9 in the
five-cent, almost identical to the current cupronickel.
Conductivity

The Mint tested six batches of five random 80/20B planchets for their conductivity. The
planchets were tested at four different frequencies, and from the lowest to the highest
frequencies, 80/20B yielded IACS readings of 5.61% to 6.93%. Deviations among the pieces
tested at each frequency were well within acceptable parameters. The readings were very
similar to current conductivity measurements.
Wear Test

As in the variability lot wear test, 80/20B wear rate was comparable to the current material,
losing 7 percent less material (17.6mg v. 19mg). In addition, the five-cent pieces showed an
average edge deformation lower than that shown by the current material. (The full test
results are available in Appendix 10.4.3.)

92

3.4.8. 80/20B Down-Selection

Environmental Impact

Comparable or Better. 80/20B has nearly the same configuration as the current five-cent,
and the addition of manganese does not cause any significant environmental impact.
Supply Chain

Comparable or Better. All the raw materials in 80/20B are in adequate supply. The number
of established suppliers is identical to the current two suppliers for the five-cent.
Coinability

Comparable or Better. Pre-production strikes of standard-crown dies at comparable tonnage
to the current strike force saw a slightly lesser rate of failure to the dies than seen with
current materials. The Mint also observed acceptable fill rates at comparable tonnage to the
current material.
Recyclability

Comparable or Better. 80/20B sees a comparable recycling option compared with current
materials for the five-cent. If this material is also chosen to replace the cladding in the clad
denominations, then the inclusion of manganese may impact the recycling options.
Durability

Comparable or Better. The Mint observed a comparable wear rate and minimal discoloration
with 80/20B. 80/20B showed a wear rate of only 18 percent, below the maximum 20 percent
set by the Mint.
Counterfeit/Slug Vulnerability (Quarter-Dollar Only)

Comparable or Better. If 80/20B is chosen to replace the cladding on U.S. clad coins, its
unique EMS will combine with the clad configuration to provide a similar level of security as
that found in the current materials.
Feasibility

Five-Cent – Feasible

93

This page intentionally left blank.

94

4. U.S. Coin Security
4.1.

Threats

In coinage, there are two threats: counterfeiting and fraud. Both can create problems for
vendors and shop owners, as well as public mistrust in coins.
4.1.1. Counterfeiting
Counterfeit coins are imitations that are passed off fraudulently or deceptively as genuine
coins. In practice, they are easily rejected by mechanical coin validators as the EMS is
incorrect, but in person-to-person commerce, they can be easily mistaken for genuine
coinage. The fake coin is almost always of little or no value.
Sometimes, coins from other countries, which look similar to U.S. coins, enter circulation.
Canadian quarter-dollars are one example. This becomes problematic when legitimate coins
(with a low value) from one country are accepted in another country as a higher-value coin.
In 2006, the Philippine 1-peso (value of 2.4 U.S. cents) was discovered to be passing for the
1-dirham coin in the United Arab Emirates (value of 27.2 U.S. cents). 29 In another case in
2013, Amsterdam discovered that over 10,000 Thailand 10-baht coins (value of 23 euro cents)
had been passing for 2-euro coins in that city alone. 30
4.1.2. Fraud
Fraud involves deceitfully and purposefully replacing coinage with slugs or tokens that are
accepted by mechanical coin validators as genuine. Mechanical coin acceptors rely on
dimensions and electromagnetic signature (EMS) rather than visual recognition. In a
fraudulent scenario, the readout of the fake coin matches a genuine coin, but it may not have
the same appearance. The fraud is recognized after the fact when the vending machine is
serviced, but by then it is too late to prevent the theft. As with counterfeit coins, fraudulent
tokens are usually of little or no value. In 2004, a man in Atlanta was arrested and convicted
for defrauding the U.S. Postal Service (USPS) with 150,000 fake dimes he had made and used
in USPS stamp machines over the course of several weeks. 31

Source: http://gulfnews.com/news/gulf/uae/general/hey-presto-a-peso-s-as-good-as-a-dirham-1.38628 (Aug.
1, 2006)
30 Source: http://www.dutchamsterdam.nl/2375-amsterdam-flooded-with-thai-currency (Dec. 11, 2013)
31 Source: internal communication between the defrauded Atlanta Post Office and the U.S. Mint HQ (20042006).
29

95

Figure 4-1. Slugs and Tokens

U.S. quarter-dollar above slugs and tokens collected from vending machines

The absence of a cashier to visually authenticate a coin enables an individual (commonly
called a “fraudster”) to substitute lower-value foreign coins or other non-genuine items
(tokens or slugs) without risk. Given the anonymous nature of vending transactions, fraud is
a very real concern with coin design and materials.
4.2.

Security Features of U.S. Coinage

Coin security is based on overt and covert features. Overt features are those easily
determined through visual or quick dimensional or weight check. A cashier would look at
the coin to determine if it looks (design and color), feels (weight), and sounds like a real coin
when deposited into the cash register. A vending machine would check the diameter or
thickness and possibly the weight. Covert features, which cannot be easily validated
visually, rely on material composition or makeup. Measurement of covert features is done
through electrical circuitry or other instrumentation. As coins increase in value, more
covert features are incorporated to deter fraud.
4.2.1. Background
Vending equipment facilitates commercial transactions without a human to handle and

validate the payment. The coin acceptor mechanism that validates the authenticity of the
payment is called a discriminator. Vending equipment prior to 1963 contained rudimentary
discriminators based primarily on the physical attributes of the coinage, (size, density,
weight, etc.).
96

Common construction items like washers and conduit knockouts could be modified to trick
these rudimentary discriminators; thus, magnets were incorporated in vending equipment to
reject steel-based materials. As product costs in vending machines increased, industry
required improved methods, and discriminators needed more sophistication and complexity.
The application of miniaturization, electronic transducers, and sensing technology created an
opportunity to take coin validation to the next level in vending. Such technology led to the
development of systems to detect a coin’s EMS or conductivity, both of which can uniquely
identify a particular coin type.
Vending discriminators now vary in complexity, depending on the value of the product
served or service rendered. For example, a “canteen operation,” where product values often
exceed one dollar, allows bills, coins, and sometimes stored-value or credit card transactions.
The coin discriminators in this system will employ more advanced features. In contrast, a
laundromat, car wash or other low-value product/service vending application relies on overt
coin characteristics and may only contain a physical check of the coin (thickness and
diameter).
4.2.2. Variances in Conductivity/EMS
Conductivity is the percent IACS (International Annealed Copper Standard) for non-ferrous
alloys (see section 3.2.7). It is a ratio of a particular alloy's conductivity compared to pure

copper at 20 degrees Celsius. EMS is a measure of a material as an “eddy current” is passed
through it, providing unique values for various metallic compositions. Both EMS and
conductivity are measured at various frequencies. Unfortunately, there is no established
industry standard for what frequency to use and conductivity/EMS readings on materials
differ from frequency to frequency. This means two materials’ readings may match at one
frequency, but be different at another.
The lack of a standard frequency creates challenges in identifying a material that can display
the same EMS across the range of frequencies used in coin acceptors. For ferromagnetic
products, an additional property (material permeability) also impacts the EMS. Other
components of coin acceptor discriminators relate to coins’ physical dimensions, specifically,
inductive thickness, an electrical reading based on the actual thickness of a specific alloy.
Vending discriminators must also accept a range of coin properties and conditions but also
screen out foreign coins, tokens, and slugs. However, the physical properties of coins can
vary based on age, use, and manufacturing tolerances. Coins with more wear have less
material and this affects the coins’ measurements. A coin that is used, for example, in
97

vending or casino operations will see more physical wear than one that is cycled through the
banking system or a coin that sits in a consumer’s jar for years. A tolerance band is set up for
the various properties being measured and periodically adjusted to accommodate the coins in
circulation. Many coin acceptors can be adjusted through software or a programming service
call, but older ones still require physical modification. A change in composition or physical
dimensions will affect the various vending segments differently and the impact will be
immediately felt by industry.
4.2.3. Coin Construction
Up to 1964, U.S. coinage for the dime and higher denominations were 90 percent silver. As
silver supplies dwindled and metal costs rose, the U.S. government changed the metal

composition. The new coinage material consisted of a pure copper core with a silver-colored
nickel/copper alloy skin. The skin was applied to the core through a mechanical process
called cladding in which the different materials were rolled and reduced in thickness under
pressure, bonding the materials together. The Mint punches coin blanks or planchets from
sheets of clad material and presses (cold forms or “coins”) the planchets into coins with the
appropriate dies. The result are clad coins with multiple layers.
By applying different signals through the sensing circuits in the coin acceptor discriminator,
sensors can see through the cladding layer and detect the core composition yielding two
separate and distinct signals for use in discrimination. Thus, the new clad material provided
increased security in coinage, both from the physical dimensions (diameter and thickness)
and from the metallic composition (skin and core metallic makeup).
The rising cost of raw materials is creating a challenge for world mints, driving them to use
lower-cost metals. Sensitive to the needs of commerce (banking and vending), national
governments must weigh the benefit of making the material change versus the impact to
industry. Some have gravitated to using iron or steel as a substrate which complicates the
security of discriminators in vending equipment. Magnets, which were used to screen out
common items, cannot be used if coins themselves are ferromagnetic. Also, due to the
abundance of steel items that can be modified to fit into vending equipment (conduit
knockouts, washers, etc.), steel is considered to present a higher level of fraud in vending. As
such, most countries consider steel viable for use in low-value coinage only.
4.2.4. Coin Security Evolution
As world mints evolve and introduce higher-value coinage systems, fraud potential increases,

and more sophisticated security systems are necessary to deter fraudsters. New technologies
98

are being developed by, or in conjunction with, world mints incorporating acoustical, optical
or micro-text signatures. These technologies are generally proprietary and are just being
considered for use in major coinage systems.
For example, The Royal Mint has developed and patented a technology termed “iSIS.” The
technology is based on introducing a fluoroluminescent compound into the plated layer that
is detected by a proprietary sensor. The measured density of the compound particles is used
to validate the coin. Another advanced technology developed by the Mint of Finland is
called “CoinTune.” This proprietary technology is based on developing a unique acoustical
signature of a coin and subsequently reading this signature in vending to validate the coin.
Finally, the Royal Canadian Mint has developed a micro-text/engraving process that provides
a unique and difficult to reproduce optical signature on the coin face. It also has developed
what it terms “DNA Mapping,” which maps and stores the unique morphology on a specific
location of the coin surface for future reference and validation. This “signature” is unique on
each coin produced and enables RM to verify or authenticate the coin.
The viability of incorporating such technologies into vending equipment has yet to be
quantified and is subject to factors such as cost, complexity, and maintenance requirements.
In discussions with various coin acceptor manufacturers, there is no active program to
incorporate any of these new technologies into existing coin acceptors. With time to be
allotted for design, marketing, and transition by the vending industry, this would place any
change in the sensor base on a five-year or greater horizon. Until such a time that these new
technologies are proven cost-effective and reliable in application, the electromagnetic
signature of clad and non-ferrous materials represents the security benchmark for coinage
alloys in automated vending operations.
4.3.

Steel-Based Coin Security

During the course of Phase II, the Mint worked closely with several, large coin acceptor
manufacturers—Cummins Allison, MEI, SCAN COIN and Coinstar—to test and analyze
struck pieces. The Mint also communicated with U.S.-based manufacturer CoinCo and
obtained its feedback. 32 These are the main companies that produce the coin-accepting
mechanisms used in vending machines within the United States and worldwide.

CoinCo tested materials in Phase I, but did not have the available time or resources to support testing in
Phase II.

32

99

As a primary reference document, the Mint used The Coin Design Handbook, version 2
(2012) prepared by the European Vending Association (EVA). 33 This document was written
by the following EVA member companies: CoinCo, MEI Conlux, NGZ, NRI (part of Crane
Payment Solutions), and SCAN COIN. In addition, it was endorsed by a number of the EVA
Coin Group member companies including Cummins Allison. Given the extensive
international involvement, it was considered a valuable reference document in evaluating
coin materials and designs for both compatibility with coin accepting mechanisms and also
security.
In the Handbook, the EVA defines Security as, “A coin that does not misvalidate, is able to be
differentiated correctly, is not easy to fraud, and has a low fraud risk, is regarded as being
more secure and suitable for higher value coins.” 34 Key considerations include the similarity
to other, lesser-valued, world coins and the ease of creating fraudulent coins, including
knowledge of techniques, and availability of equipment and materials. Complex machining,
unique or expensive equipment, and materials that are more difficult to obtain provide
increased protection against fraud. According to the EVA, “Fraud coins that are very simple
to manufacture and use widely available materials can present a very real fraud risk to
relatively low value coins.”34
The EVA further defines coins by their value using the Euro as the basis. Coins are
characterized in Table 4-1, below.

Table 4-1.

EVA Coin Value Categories

Category

Value

Very Low Value

up to 2 cents Euro or equivalent (up to approx. 2.7¢ U.S.) 35

Low Value

>2 cents Euro to 20 cent Euro or equivalent (>2.7¢ to approx. 27¢ U.S.)

Medium Value

>20 cents Euro to 50 cents Euro or equivalent (>27¢ to approx. 68¢ U.S.)

High Value

>50 cents Euro or equivalent (>68¢ U.S.)

Previously known as the World Vending Association, founded by the U.S.-based National Automatic
Merchandising Association and the EVA.
34 Emphasis EVA’s.
35 Using an exchange rate of 1 Euro = $ 1.357.
33

100

The level of a coin’s security is directly related to its value. Stated differently, the level of
security (and cost associated) should be commensurate with the coins value to effectively
support commerce. Fraudsters and counterfeiters are drawn to higher-value coins, with a
greater return for their effort.
Steel-based coinage materials considered in Phase II include plated steel and stainless steel.
The Mint tested plated steel in two versions: nickel-plated steel obtained from The Royal
Mint and multi-ply-plated steel obtained from the Royal Canadian Mint. These are single or
multiple layers of nickel and copper/nickel plated on a cold-rolled, low-carbon steel core.
They are used in coinage worldwide. The Mint worked with an external research firm to
test different grades of stainless steel.
4.3.1. Plated Steel
When discussing coin security vs. construction, the EVA Handbook notes:
Single Layer (i.e. Nickel-Plated Steel)

Plated coins that have a single plated layer on a solid steel core are effected by
the variability in the manufacturing process and the dominant effects of the
core. (page 28)
The risk from fraud is high due to the ready availability of round steel discs. As
well as widespread availability of Copper and Nickel plating facilities
worldwide. (page 28)
Single layer plated coins should only be used for low value coins because of
the ease of and risk from fraud. (page 28)
Multi-Layer Plated Coins

The risk from fraud is high due to the ready availability of round steel discs. As
well as widespread availability of Copper and Nickel plating facilities
worldwide. (page 30)
Although multilayer plated coins enable other single layer plated steel coins
that have a similar diameter and thickness to be differentiated, they have a
high risk from fraud because of their steel and copper/nickel plated
construction. Overall they offer no improvements in security using inductive
material sensors in today’s coin validators when compared to single plated
layer. (page 30)

101

Multilayer plated coins should only be used for low value coins because of the
ease of and risk from fraud. (page 30)
Ferromagnetism

Steel is ferromagnetic (attracted by a magnet), which presents several problems in coin
acceptor security. Phase I identified vending machines and laundromat facilities as being the
dominant shareholders for automated point-of-sale transactions. These machines have a
magnetic discriminator intended to capture steel slugs, which would need to be removed or
disabled to accommodate steel coins.
Foreign Coins

Although plated-steel coins would cost less to produce, they are also more vulnerable to
fraud. Several examples of foreign plated-steel coins show the relationship between
construction, coin value, the EVA guidelines, and equivalent U.S. values.

Table 4-2.
Country/Region

Canada

United Kingdom

European Union

Foreign Plated-Steel Coins

U.S.
Equivalent
5-cent
low value
4.6 cents
10-cent
low value
9.2 cents
25-cent
low value
23 cents
50-cent
medium value
46 cents
1-dollar
high value
92 cents
2-dollar
high value
184 cents
5-pence
low value
8.5 cents
10-pence
low value
17 cents
Note: 20-pence through 1-pound are monolithic alloy
construction (non-steel). Higher is non-steel bi-metallic.
1-cent
very low value
1.36 cents
2-cent
very low value
2.74 cents
5-cent
low value
6.8 cents
Note: 10-cent through 50-cent are monolithic alloy
construction (non-steel). Higher are non-steel bi-metallic.
Denominations

EVA Coin Value

The majority of mints conform to the EVA guidelines and only use plated coins for lowvalue denominations (i.e., below approximately 27¢ U.S.). The Royal Canadian Mint,
however, utilizes plated materials for low-, medium- and high-value denominations. In
separate discussions, neither The Royal Mint nor the Royal Canadian Mint claims to
experience fraud with their plated coins, though the RCM employs many security features
(such as laser-etching a micro-engraved image of a maple leaf on their one-dollar coin). The
Royal Canadian Mint and The Royal Mint (as well as other international mints) also have
102

active research programs in anti-fraud techniques to improve the security of their platedsteel coins.
While the UK and Canada claim not to experience significant counterfeiting with their
plated-steel coins, many examples of counterfeiting are reported in China, which uses nickelplated steel coins. In 1991, China began to use nickel-plated steel on its one-Yuan coins.
The core is low-carbon steel and surface is plated with pure nickel. Because the common
core materials cost very little, and nickel plating is an inexpensive, simple process, there have
been tens of millions of counterfeit one-Yuan coins circulating since the coins’ release. The
total cost for making a single, fake, one-Yuan coin is about 3 U.S. cents.
The following table shows a partial list of seized counterfeit one-Yuan coins; these were
published in Chinese newspapers. More counterfeit coins are still circulating, and as a result,
many small shops in China no longer accept one-Yuan coins in commerce.

Table 4-3.

Counterfeit Seizures in China

Date

Location

Quantity

2006 May

Nanchang

10,000,000

2006 August

Heibei Province

10,520,000

2007 December

Nanjin

30,000,000

2008 November

Fuzhou

700,000

2009 August

Feishan

220,000

2009 August

Zhengzhou

100,000

2009 September

Hefei

1,000,000

4.3.2. Stainless Steel
Stainless steel is being considered as an alternative metal for U.S. coinage. It is termed
monolithic or homogeneous since it consists solely of one alloy and exhibits the same

chemical composition throughout. Stainless steel is produced in two forms: ferritic (400
series) and austenitic (200 and 300 series), both of which are an alloy of iron and chromium.
Ferritic stainless steel has very little nickel and therefore has lower material costs. It is
ferromagnetic, which means it is attracted by a magnet. This presents several problems in
vending security. First, many coin acceptors used in vending and the laundromat industry
103

have a magnetic discriminator intended to capture steel slugs; this would need to be removed
or disabled to accommodate ferritic steel coins. Second, the ferritic steel’s EMS is highly
variable and influenced by manufacturing inconsistencies and by the handling of a coin over
time. This requires coin acceptors to undergo modifications to have a wider acceptance
band, making the material less secure when used in coin validators.
Austenitic stainless steel has a significant quantity of nickel (which makes it nonferromagnetic), so it has a higher material cost. The EMS of austenitic steel does not vary
much from alloy to alloy, though, which means a coin validator cannot effectively
discriminate between one austenitic stainless steel grade and another.
4.3.3. Homogeneous Materials
For both ferritic and austenitic stainless steels, the EVA Handbook notes that:

Non-magnetic homogeneous coins are generally to be considered for low to
medium value denominations; however the security of the coin depends
significantly on the choice of material.
If the homogeneous material is commonly available and/or cheap, the risk of fraud is greater
because there is no unique construction in homogeneous coins or special EMS to help
discriminate real coins from frauds. Stainless steel’s readily available material and solid
construction enables someone to easily manufacture a disc that could be used in vending.
For low-value coins, this is not a significant risk as the return on investment does not offset
the fraudster’s time and costs in manufacturing the fakes. Risk becomes greater at higher
denominations, where there is more return on investment.
4.3.4. Coin Sorter/Validator Testing
Although each coin acceptor manufacturer has a different algorithm and frequency in their

mechanisms, each measures the conductivity of coins. The “accept” range of these

mechanisms’ sensors (the “band width,” or “window”) is of particular concern in coin
security. If two compositions of the same coin/denomination have very different EMSs, the
mechanism needs to be set to accept both, which means its window of acceptance opens very
wide, leaving it more vulnerable to being defrauded by slugs and tokens that could easily fall
inside the window.
The Mint used an industry-standard coin sorter/validator (CSV) to capture data of various
materials being tested and considered. The Mint compared the internal test results of various

104

materials which compared the spread in both the Outer Conductivity (OC) and Inner
Conductivity (IC).
The CSV sensors change their frequency to read the coin only partially under the surface,
and then read the same coin more deeply, to gather the entire EMS of the material. As coins
pass through, some variability is seen. In testing, for the current cupronickel, the sensor
readings and their variability was recorded, giving an average value for each of the criteria
with the variance on each criterion.
The CSV was programmed with acceptance windows pre-set for each EMS parameter. The
acceptance window width was based on the variance of actual coins, either newly minted or
pulled from circulating coinage. The Mint’s coin validation involved comparing the
measured value of each EMS parameter to the acceptance windows for coin validation.
The plated-steel materials’ criteria for the five-cent pieces differed drastically from the
current material, having some scores 12 percent higher, and others over 50 percent lower
than the current material. Most of the criteria had a variance at least 10 percent higher than
the average score. For inner and outer conductivity, the variance for NPS and MPPS was
over 33 percent of the average score, as compared with just over 10 percent variance on the
current material.
The Mint made the following findings from this test:
1. Plated-steel EMS ranges are wider than those of the current material, necessitating
wider acceptance windows and therefore less security.
2. Plated-steel and monolithic EMS ranges tend to overlap at multiple frequencies,
diminishing the enhanced security of dual-frequency coin validation.
3. Clad construction offers high security, as evidenced by the low incidence of EMS
overlap with MPPS and NPS. These findings are in line with EVA’s Coin Design
Handbook’s rating of clad construction being more secure than plated.
4. Clad constructions may have relatively large EMS range widths, but security is not
compromised because EMS average values are widely separated when validated using
dual-frequency acceptors.
The complete readings are available in Appendix 10.9.

105

4.4.

Steel-Based Coin Security Conclusions

Given the EVA guidelines, it is clear that steel coin construction would present acceptable
risks for application on the United States five-cent and dime (low-value denominations).
While the quarter-dollar is technically below the EVA-recommended threshold, it is very
close, and that status is sensitive to variations in the exchange rate (since the EVA guidelines
are based on the Euro). Of greater consideration in the United States is the fact that the
quarter-dollar is the highest-value coin used regularly in vending transactions. This means
that the risk of fraud on this denomination needs to be seriously considered in this country
more so than others. While ultimately a policy decision (risk vs. return), the application of
plated-steel material to the quarter-dollar is not advisable from a technical perspective. The
material gains must be weighed against the impact of fraud and its effect on the confidence of
the monetary system in supporting commerce.
Use of stainless steel for the five-cent or the dime (not both) would be acceptable from a
security standpoint; use of stainless steel would not be acceptable for the quarter-dollar. One
unique consideration with homogeneous coin construction is the relative size of the
denominations. In most of the world’s coin sets, the size of the coin increases as the value
does. This means a lower-valued coin could not be made into a higher-valued one by rolling
or resizing. In the U.S., the larger size of the five-cent vs. the dime (a legacy of the relative
value of cupronickel vs. silver) would allow this practice, and so precludes the use of the
same monolithic material on both the five-cent and the dime.

106

5. Coinability
Coinability is a subjective characteristic, but a critical one when evaluating potential
materials for coining. It is the term associated with how readily a material can be struck into
a coin and encompasses a number of elements including material mechanical properties,
blank preparation/lubrication, upset profile 36, level of details in the coin design, height of
details in the design (i.e. height of relief 37 and crown 38), and die surface finish. Each of these
elements contributes in varying degrees to the performance of a material during high-speed
stamping. Throughout testing, the Mint expended significant effort to keep these elements
consistent from material to material.
When evaluating a potential material, a balance must be achieved between keeping the
elements consistent with other material testing (to attribute the outcome to the alternative
material) and optimizing the above elements for each material (as they act as a “system”
coming together to produce a result). For the purposes of consistency, the main focus was on
using the same die design, stamping press, and quality standard.
5.1.

Testing Methods

Two methods were used to evaluate coinability: progressions strikes 39 and extended striking
trials (pre-production runs) in which die pairs were run to failure. Acceptable quality was
determined through initial progression strikes on the material in which coin fill and
dimensions were evaluated with increasing striking force and an aim striking tonnage set
that provided acceptable visual and dimensional results.
Over the course of pre-production runs, the dimensions and appearance of the struck pieces
were checked frequently with the quality standards being the same as those used in normal
production operations for circulating coins. Circulating coins are not free from defects, but
the coins must be within dimensional tolerances and observed defects must be limited in

Upset refers to movement of metal on the edge to pre-form the rim.
Height of relief is dimension of highest part of the artwork as referenced from the lowest part of the field
adjacent to the artwork.
38 Crown is the dimension that characterizes the depth of the basin before the artwork is overlaid.
39 Progression strikes are a controlled test where the striking force is incrementally increased and the
development of the design fill, edge profile, and coin dimensions are closely examined to evaluate a material.
In addition, an aim striking force (tonnage) is established that provides an acceptable level of visual quality and
dimensional compliance.
36
37

107

size. The resultant average for die life and the level/degree of defects observed in the die and
struck piece were the basis for determining coinability. A rating of Comparable or Better
(than the current material) or Less than Current was determined and used as one of the
down-select criteria.
The Martha Washington nonsense design was patterned exactly after the current designs
used for circulating coins with similar images (Martha Washington instead of Thomas
Jefferson on the five-cent or George Washington on the quarter-dollar obverse and Mount
Vernon vs. Monticello on the reverse of the five-cent) and similar inscriptions (same letters,
but jumbled). As it was known that U.S. coin designs have more detail and relief than most
circulating world coins, two alternatives were developed to the standard-crown nonsense
dies. These were half-crown and flat-crown in which the nonsense design details were kept
identical, but the height of relief and crown were reduced by half (half-crown) and then
again by half (flat-crown) to provide dies that more closely approximated international
coinage. Pre-production runs were performed on the current material for both the standard
and the modified dies so there would be a valid baseline.
5.2.

Baseline Results

Obtaining a statistically valid die life for alternative materials would require a significant
number of runs. To evaluate coinability on candidate materials, the Mint decided to run at
least four die pairs to failure or 500,000 strikes, whichever came first. A target of 500,000
strikes was established because that represented an acceptable productivity threshold for die
life and was representative of past results on the five-cent and quarter-dollar circulating
coins (see section 1.5).
Tables 5-1 and 5-2, below, respectively show the results of the baseline run on the current
five-cent and quarter-dollar materials. Each die pair consisted of an obverse die and a
reverse die. If one die in a pair failed, both were then replaced.

108

Table 5-1.

Baseline Die-Life Determination (Five-Cent)

Crown

Die Life
(strikes)

1st

Standard

365,672

Crack and piece out on reverse

2nd

Standard

500,003

No objectionable defects

3rd

Standard

500,031

4th

Standard

641,116

5th

Half

500,000

No objectionable defects noted

6th

Half

500,003

Slight crack developing at top of
bonnet

7th

Half

500,350

No objectionable defects noted

8th

Half

503,256

No objectionable defects noted

9th

Flat

500,037

No objectionable defects noted

Die Pair

Failure Mode

Crack observed on bonnet and
weakness in steps on reverse; was
borderline to continue
No objectionable defects ran until
641,116 and retired dies

10th

Flat

458,247

Piece out noted on reverse before
200,000, not significant enough to
pull the die. 2nd piece out noted on
reverse still acceptable for
circulating quality. 3rd piece out
observed and dies pulled.

11th

Flat

500,126

No objectionable defects noted

12th

Flat

467,655

Piece out noted on reverse (letter S)

Overall

5,936,496

Average 494,708

These results validated that the Martha Washington nonsense dies were representative of the
normal circulating dies in that they displayed similar defect patterns and life.
The results of the baseline run on current quarter-dollar material with half- and standardcrown dies are in the following table.

109

Table 5-2.

Baseline Die-Life Determination (Quarter-Dollar)
Crown

Die Life
(strikes)

1st

Standard

500,028

No objectionable defects noted

2nd

Standard

500,004

No objectionable defects noted

3rd

Standard

459,075

Crack on obverse near base of
Martha’s bust

4th

Standard

500,002

No objectionable defects noted

5th

Half

500,000

No objectionable defects noted

6th

Half

501,856

No objectionable defects noted

7th

Half

500,000

No objectionable defects noted

311,601*

Defect noted on obverse, die retired.
Under further examination, “defect”
was an impression from debris
stamped into the surface; no actual
defect in die.

3,460,965

Average 494,424

Die Pair

8th

Overall

Half

Failure Mode

* - Die retired prematurely; not counted toward overall or average.

Again, the results both validated the use of the Martha Washington nonsense dies as
representative of circulating results and the use of 500,000 as a target threshold.
5.2.1. 80/20B Five-Cent
The upset profile on the material provided for the pre-production run was similar to that

used for the circulating five-cent. Procedures for annealing and blank preparation (including
chemicals currently used) were provided to the vendor. The Mint does not have any large
capacity capability for annealing or preparing blanks without risking contamination with
current material, so external processing was necessary. Progression strikes set aim tonnage at
54 tonnes.

110

Table 5-3.
Die Pair

Initial 80/20B Die Life (Five-Cent)

Die Life (strikes)

1st

<100,000, but ran to
500,000

2nd

<100,000, but ran to
255,274

3rd

67,413

4th

116,130

5th

64,574+

Overall

1,005,391 (603,391)

Failure Mode
Significant wear noticed on both sides before
20,000, would have retired before 100,000 but
continued run to 500,000. Engraver initials worn
on the obverse around 200,000. Cracks noticed in
the bonnet area around 400,000 strikes. Cracking
more prevalent, especially on the obverse letters.
Wear noticed on reverse starting at 12,000 strikes.
Cracking noticed in the bonnet area around
200,000 strikes. Excessive die wear seen, but
elected to continue to observe other defects.
Wear observed on outer perimeter of struck piece
by 10,000 strikes. Noticeable wear at 20,000
strikes on both sides. Wear marks developing near
nose on the obverse at 40,000. Dies retired when
wear was deemed excessive visually.
Same pattern of wear developing by 20,000 strikes
including the nose area. Retired dies due to
excessive wear.
Material burnished using standard circulating
chemicals. Ran available material, no noticeable
wear and die pair could have been run much
longer.
Average 120,678

The 80/20 material is very close in composition to the current cupronickel (75% copper, 25%
nickel). There is a larger quantity of manganese in the 80/20 to match the EMS of the fivecent, approximately 4% Mn vs. less than 0.6% in the current material. The manganese level
is similar to the level in the dollar coin material which does not exhibit excessive die wear, so
the difference in manganese is not felt to be a contributor to the excessive die wear. Given
that, the material’s performance was not considered representative. The Mint associated the
premature wear issue with the blank cleaning/lubrication being significantly different than
that on our standard cupronickel.
On a conference call with the supplier, the Mint learned the desired lubricant chemical had
not been applied and, in fact, there was only a tarnish inhibitor applied to the blanks, no
lubrication. This was confirmed when a small quantity of the 80/20B blanks were burnished
in the small-volume burnishing machine in the R&D room. The Mint then struck the newly
burnished material with normal appearance through over 60,000 strikes (see 5th die pair in

111

Table 5-3, above). Wear had been noticed consistently before 20,000 strikes on the
untreated material.
Coinability and die life of the 80/20B cannot be definitively assessed on these results. The
excessive die wear is considered to be related to the inadequate blank preparation,
specifically no lubrication. The remaining material was returned for proper blank
preparation and the pre-production run resumed on July 14, 2014.
Testing resumed when the Mint received the treated material. There were some issues with
the feed fingers during the tests, but this was unrelated to the material, and was not counted
against the material. On the two die pairs that did not have problems with the feed fingers,
die life was comparable to the current material, although when the dies failed with 80/20B, it
was the reverse die that failed, as opposed to the current material seeing die failure on the
obverse.

Table 5-3.
Die Pair

Treated 80/20B Die Life (Five-Cent)

Die Life (strikes)

Failure Mode

1st

454,000

No objectionable defects noted

2nd

1,095*

Die clash on fingers; retired and installed die pair #3

3rd

470,000

No objectionable defects noted

4th

---*

Die clash on fingers before start; replaced with die
pair #5

5th

47,931*

Problems continued with fingers; ended preproduction run and emptied the feed hopper

Overall

924,000

Average 462,000

* - Die retired prematurely; not counted toward overall or average.

112

5.2.2. Multi-Ply-Plated Steel (Five-Cent)
The Mint used the Canadian-standard upset profile provided by RCM. Due to the abrasive

nature of the nickel surface, protective die coatings were required. This is not a practice the
Mint uses except for numismatic coins, so the dies were sent to the RCM for coating with
their Physical Vapor Deposition (PVD) process and recipe. As their practice was to polish
the die surface before coating, some dies were coated without polishing and others with to
provide results that would guide future practices. For the pre-production runs, the Mint
only used the polished dies which were buffed after PVD coating.
Blank surfaces were prepared per the standard practice the RCM uses on its coinage and the
material they provide to other world mints. Progression strikes of standard-crown test dies
showed non-fill in high-relief areas (i.e., Martha’s bonnet) at up to 60 tonnes, well above the
normal circulating strike tonnage of 54 tonnes. The decision was made to use 54 tonnes as
the aim tonnage for standard-crown dies. Aim tonnage for the half-crown dies was set at 52
tonnes.

113

Table 5-4.
Die Pair

MPPS Die Life (Five-Cent)

Crown

Die Life (strikes)

Failure Mode

1st

Standard Not
Polished

125,779

2nd

Standard Not
Polished

Crack noticed on bonnet on obverse at
100,000. Crack started at 20,000 strikes.
Die retired due to obverse crack.

67,121

Crack on obverse

3rd

Half Polished

267,000
(500,146)

4th

Half Polished

138,568

5th

Half Polished

103,310

6th

Half Polished

108,517

Overall

At 194,000 strikes, noticed defect on the
nose (Obverse). At 267,000 strikes the
defect was significant enough that the
die should have been retired. Continued
running to see what additional defects
would manifest. At 442,000 piece-outs
seen on reverse near the letter F. Ended
run after 500,000 strikes.
Retired die due to crack in nose area of
the obverse
At 40,000 strikes noticed the die coating
starting to fail, continued run until crack
or piece out. Pulled die at 103,310 for
excessive tool marks and coating failure
on the obverse.
Crack on nose seen at 89,000. Stopped
run at 108,517 due to crack on obverse.

810,295
(1,043,441)

Average of 135,049 strikes

Pre-production strikes of standard crown dies were conducted at tonnage comparable to that
used for the current material, although given that the features were not optimized for this
material and lack of fill was observed in high-relief areas on the obverse design. Preproduction strikes using half-crown dies were conducted at lower tonnage than current
strike tonnage.
Coin edge thickness was within specifications, but measurably greater than current coins
struck at higher tonnage. Multi-Ply Plated Steel five-cent exhibited premature die
retirements as compared to the baseline. Defects seen included cracks, tool marks, and die
coating failures. The coating failures are felt to be related to metal oxides on the dies
surfaces. PVD coatings typically do not adhere as well to metal oxides as elemental metal.
The cracks were present on both the Standard Crown and Half-Crown Martha Washington
designs, which illustrates that the feature changes necessary to accommodate plated-steel
material would not just be a lowering of the relief/crown.

114

More feature changes would be required. Improvement in coinability and die life could be
possible with an optimization of the Martha Washington designs to be more compatible with
the MPPS. This would include a softening of detail, adjustments in the height and degree of
image detail, as well as adjustments to the lettering. These changes would not affect the
public recognition, but would diminish the aesthetics of the circulating coin appearance.
There is a significant gap though between the averages of 135K and the desired baseline
performance of 500K so it is unlikely that the design and/or upset profile changes alone will
close the die-life gap fully; therefore, some reduction in die life is to be expected with this
alternative material. This is confirmed by RCM’s experience of 350K die life on their fivecent coin. Given the feature changes and lower anticipated die life, this material should be
considered as feasible, but Less than Current in coinability and die wear.
5.2.3. Multi-Ply Plated Steel Quarter-Dollar
The upset profile provided was RCM 3M with angle A40 moved closer to the blank edge to

address the concentric ring observed on test pieces stamped from previous variability lot
planchets. As with the five-cent, the nonsense dies were sent to the RCM for coating to

protect against the increased wear encountered from the nickel. Blank surface preparation
was per the standard practice the RCM uses on its coinage and the material they provide to
other world mints. Progression strikes set aim tonnage at 64 tonnes for the standard crown
and 62 tonnes for the half-crown.

Angle of the top edge of the upset with respect to the flat surface on a drawing that shows the exact upset
profile from a side-view.

40

115

Table 5-5.
Die Pair

MPPS Die Life (Quarter-Dollar)

Crown

Die Life (strikes)

1st

Standard Not
Polished

152,179

2nd

Standard Not
Polished

242,682

3rd

Half Polished

106,036

4th

Half Polished

155,957

5th

Half Polished

318,986

6th

Standard not
polished

231,344

7th

Standard not
polished

150,030

8th

Half not
polished

140,304

Overall

Failure Mode
Noticed crack on bonnet at 20,000 under
microscope, continue to run, retired from
service due to coating failure.
At 180,000 noticed small mark on
obverse chin and start of crack on
bonnet. Retired dies due to crack on
bonnet.
Noticed a “glow” appearance on both
sides of the pieces soon after start-up.
Noticed crack on reverse in the rhino’s
body at 76K. At 80K, rev crack getting
larger and crack starting in obverse
bonnet area. Retired dies due to cracks
on both sides.
Still see a “glow” on both sides of the
pieces after start-up. Defect starting on
the obverse chin area at 27K. Crack
developing on reverse in the rhino body.
Retired dies due to cracks on both sides.
Crack starting on obverse in the bonnet
area at 215K, cracks noticed on the
reverse in the mountain field at 250K.
Retired dies due to crack on obverse
bonnet area.
Crack starting in obverse bonnet area at
102K. Retired dies due to obverse crack
and delaminated coating.
Noticed coating peeling at 125K lower
bust area, retired dies due to coating
failure.
Retired due to coating failure in the
obverse field area.
Standard Crown 194,059
(Half-Crown 180,321)

776,235
(721,283)

Tonnage was comparable to that used for the current material, although given the features
were not optimized for this material, a balancing was needed between desired coin fill and
dimensions. Multi-Ply Plated Steel exhibited premature die retirements as compared to the
baseline. Defects seen included cracks, tool marks, and die coating failures. The coating
failures are felt to be related to metal oxides on the dies surfaces. PVD coatings typically do
not adhere as well to metal oxides as elemental metal. The cracks were present on both the

116

Standard Crown and Half-Crown Martha Washington designs, which illustrates that the
design changes necessary would not just be a lowering of the relief/crown. Improvement in
coinability and die life could be possible with an optimization of the Martha Washington
designs to be more compatible with the MPPS.
The current circulating coin design will need to be modified if this material is to be used.
This would involve a lowering and softening of details in the image and lettering. This
would not affect the public recognition, but would diminish the aesthetics of the circulating
coin.
There is a significant gap between the averages of 188K and the baseline performance of
500K, so it is unlikely that the design and/or upset profile changes alone will close the die life
gap and some reduction in die life is to be expected with this alternative material. This is
confirmed by RCM’s experience of 350K on their 25-cent coin. Given the need for feature
changes and lower anticipated die life, this material should be considered as feasible, but Less
than Current in coinability and die wear.
5.2.4. Nickel-Plated Steel Five-Cent
The pre-production upset profile provided was modified based on feedback provided to The

Royal Mint after striking variability lots. Earlier variability lots exhibited premature edge

fill, which was not observed during pre-production strikes. As with the MPPS, the five-cent
nonsense dies were sent to The Royal Mint for coating to protect against the increased wear
encountered from the nickel surface. Blank surface preparation was per the standard
practice the RM uses on its coinage and the material they provide to other world mints.
Progression strikes set aim tonnage at 54 tonnes for the standard crown.

117

Table 5-6.
Die Pair

Die Prep

NPS Die Life (Five-Cent)

Die Life
(strikes)

1st

Standard;
Not polished

75,542

2nd

Standard;
Polished

252,515

3rd

Standard;
Polished

270,218

4th

Standard;
Not polished

80,001

5th

Standard;
Not polished

76,953

Overall

Failure Mode
Wear seen within the first 20,000 strikes,
especially on the reverse at the 10 and 2
position. Checked die height and was ok,
polished the die and resumed striking. Wear
marks continued and losing detail on the
reverse. Secured run due to crack on
reverse left side of building to coin edge.
28,000 strikes finger smashed and others
severely worn requiring change. Continued
feed finger and blank feeding issues. Retired
die pair due to die clash.
Feed finger and blank feed issues
encountered from the start. Coins show
wear, especially around the lettering. Crack
staring at 100,000 strikes on Obv top of
bonnet, scattered small die coating failures.
Started practice of changing fingers every
80,000 strikes. Retired die pair due to crack
on obverse in the bonnet and PVD coating
failures.
Oilers were turned on as a trial, obverse
becoming shiny; reverse still shows a matte
finish. Widespread wear noted at 67,000
strikes on obverse and increasing wear on
reverse. Numerous coating failures and
crack starting in nose. Retired die due to
excessive wear.
Conducted strikes with oilers off. Obverse
die worn in a manner similar to the 1st “not
polished” die pair and did not become shiny
as the 4th die pair with oilers on. Dies retired
due to excessive wear.
Overall average of 151,046 strikes
Not Polished 77, 499 strikes
Polished 261,367 strikes

755,229

Tonnage was comparable to that used for the current material with both fill and dimensions
acceptable. Nickel-plated steel exhibited premature die retirements though as compared to
the baseline. Defects seen included cracks, excessive wear, tool marks and die coating
failures. The coating failures are felt to be related to metal oxides on the dies surfaces. PVD
coatings typically do not adhere as well to metal oxides as elemental metal.

118

The cracks were present on both the Obverse (bonnet area) and Reverse (building top corner
to coin edge). A significant difference was seen between the Not Polished and Polished die
life indicating that going forward circulating dies would need to be polished to provide a
more uniform surface and one that was free of oxides.
The planchets and struck pieces exhibited indications of poor lubrication (severe bridging in
the feed hopper and Kuster Cart) and that needs to be investigated further with the RM. The
excessive wear on the press parts, is unacceptable and must be resolved to support sustained
coining operations. Improvement in coinability and die life could be possible with an
optimization of the Martha Washington designs to be more compatible with the NPS.
The hardness check on the retained planchets showed the NPS material to be about 20
percent harder than the current material and harder than the RCM plated steel. Also the
upset profile appeared sharper vs. the current material’s flatter configuration. Both of which,
along with the poor lubrication, could also have contributed to the excessive wear. Most
definitely there would need to be some accommodation with the current circulating coin
design images and features if this material was to be used. The design changes would not
affect the public recognition, but would diminish the circulating coin’s aesthetics. The blank
lubrication and part wear also needs to be addressed to make the material viable.
Since the material is utilized in the United Kingdom and many other countries this is
possible, but will require optimization trials. There is a significant gap though between the
averages of 261K on the polished coated dies and the baseline performance of 500K so while
it is possible to double the die life with changes in features and lubrication; it is not likely
that these changes alone will close the die life gap and some reduction in die life is to be
expected with this alternative material. The experience of the RM is around 600K strikes for
the 5-pence and 10-pence. Experience with other countries they have supplied reflected an
average of 447K strikes with a range from 215K to 800K. This average is on coins with very
differing designs and the quality standards for those Mints are not known.
Given the need for feature changes and lower anticipated die life, this material should be
considered as feasible, but Less than Current in coinability and die wear.
5.2.5. Nickel-Plated Steel Quarter-Dollar
The pre-production upset profile provided was modified based on feedback provided to The
Royal Mint after striking variability lots. Strike tonnage was higher than the current

material and die life on both standard and half crown was noticeably less. Use of coated and

119

polished dies was necessary. While improvement could be expected with further
optimization of coinage system; obtaining a die life comparable to the current material is not
likely. Coinability should be considered Less than Current.

120

Table 5-7.
Die Pair

Die Prep

NPS Die Life (Quarter-Dollar)

Die Life
(strikes)

1st

Standard
Polished

145,919

2nd

Standard
Polished

105,236

3rd

Standard
Polished

54,264

4th

Standard
Polished

57,907

5th

Half Crown
Polished

86,240

6th

Half Crown
Polished

101,000

7th

Half Crown
Polished

102,600
(127,991)

Overall

Failure Mode
Crack on obv, bottom of bust, was noticed
early at 20,000 strikes and later progressed to
objectionable (larger, more visible). Cracks on
obv (bottom and top of bust) and rev
(lettering). Pulled for crack at bottom of bust.
Coating delamination noticed early on, not
objectionable. Crack on obverse at 7 o’clock
position, radiating out to edge.
Die clash with feed fingers damaged dies so
curtailed run. (Not counted toward total, as
material was not cause of failure.)
Feed finger clash at 961 strikes, dies were
inspected and OK – switched to plastic fingers.
Retired die later due to crack on obverse
radiating out to border.
Coating delamination noticed after 4,000
strikes, not objectionable. Crack noticed at
top of bonnet and bottom of bust at 52K.
Retired die due to crack on bottom of the bust
getting more pronounced.
Observed crack starting on bottom of bust
around 22,000 strikes. Retired die due to
cracks at bottom of bust, also noticed crack on
Rhino body on the reverse.
At 60,000 strikes noticed crack on the bottom
of the bust (Obv) and Rhino body (rev),
continued to run. A second crack observed
developing on the Rhino body at 102,600
strikes, would have been cause for retirement,
but elected to run further. At 113,200 strikes
noted crack on obv through the letters
PROJECT that ran to the border. At 122,300
strikes noted crack in more lettering on the
obverse and decided to run out the rest of the
feed hopper.
Standard Crown average: 103,021
(Half Crown average: 96,613)

309,062
(289,840)

Progression strikes were performed on the pilot pre-production material received earlier;
performed abbreviated progression strikes to confirm correct tonnage, fill and dimensions,
aiming for 66T, but settling on 68T after observing unacceptable diameter at 66T. This was

121

related to the thicker upset profile which caused the border to completely fill before
achieving nominal coin diameter (locked border).
No excessive wear on the coated dies was noted throughout the run and there was less wear
on the feed fingers and press parts than experienced on the five-cent. The Mint encountered
feed issues throughout the run which required adjustments to the press to accommodate (had
to dress up the swivel plate and feed bowl on multiple occasions).
The Mint consistently observed cracks at the bottom of the bust on both the standard and
half-crown designs. Also encountered cracks in lettering on both sides and the body of the
rhino on the reverse. The cracks in the lettering were not observed during the baseline
strikes or on other 25-cent material struck. Ran four die pairs with standard design (one pair
clashed so wasn’t counted) average of the other three was 101,021 strikes. On the half
crown, 3 die pairs were run with an average of 96,613 strikes.

122

5.3.

Conclusions

Table 5-9.
Material

Pre-Production Average Die Life

Denomination

Aim Tonnage

Number
Die Pairs

Average Die Life

Current Standard Crown

Five-cent

54 tonnes

4

501,706

Current Half Crown

Five-cent

54 tonnes

4

501,627

Current Flat Crown

Five-cent

54 tonnes

4

481,516

80/20B No Lubrication

Five-cent

54 tonnes

5

120,678

80/20B With Lubrication

Five-cent

54 tonnes

2

462,000

Five-cent

54 tonnes

2

96,450

Five-cent

52 tonnes

4

154,349

Multi-Ply Plated Steel –
Standard Crown
Multi-Ply Plated Steel –
Half Crown

Five-cent

54 tonnes

5

Overall 151,046
Not Polished 77,499
Polished 261,367

Current Standard Crown

Quarter-dollar

62 tonnes

4

489,777

Current Half Crown

Quarter-dollar

62 tonnes

3

500,618

Quarter-dollar

64 tonnes

4

194,059

Quarter-dollar

64 tonnes

4

180,321

Quarter-dollar

68 tonnes

3

103,021

Quarter-dollar

68 tonnes

3

96,613

Nickel Plated Steel

Multi-Ply Plated Steel
Standard Crown
Multi-Ply Plated Steel
Half Crown
Nickel Plated Steel
Standard Crown
Nickel Plated Steel
Half Crown

Results from the pre-production testing support the following findings:
-

80/20 tonnage (54T) was comparable to that used for the current material, with fill and
dimensions good. Die life was also comparable as was the mode of failure (cracks). One
difference was that the reverse exhibited cracks, while on the current material the
obverse is the normal side to fail. The slight difference in composition did not affect the
coinability once proper blank treatment was applied.

-

Nickel-plated material will require polished and coated dies for circulating coin
production.

123

-

Wear resistance of press components in contact with nickel-plated materials must be
increased.

-

Plated-steel material will require changes in the design, specifically a softening of image
and lettering and lowering of detail height. These changes should not affect the public
recognition of coins, but could diminish the aesthetics of the circulating coin.

124

6. Findings/Conclusions and Recommendations
Two separate types of alternatives were considered during Phase II testing/evaluation. The
first was a material with an EMS and piece weight that was potentially seamless with the
current material. The second were co-circulate alternatives where the EMS differed from
the current material and the piece weight would vary from the current material by 4 percent
or more.
Potentially seamless alternatives would not require changes to the coin acceptors, but would
only offer modest material savings (approximately 3 percent). Co-circulate alternatives
provide much greater materials savings (20-35 percent), but would require significant
stakeholder conversion costs to accommodate the different EMS.
•

Potentially seamless alternative evaluated:

80/20

•

Co-circulate alternatives evaluated:

Nickel-plated steel (NPS)
Multi-ply-plated steel (MPPS)
Stainless steel
Copper-plated zinc (CPZ)
Tin-plated CPZ (TPCPZ)

6.1.

Findings and Conclusions

Seamless Material

1. A variant of today’s current cupronickel composition, termed 80/20, which has a
lower nickel content with higher manganese, was found to be seamless when tested
by three separate coin acceptor manufacturers. 41 The Mint estimated this material
would provide approximately $5.25M annual savings ($3.2M for the five-cent, $0.8M
for the dime, $1.25 for the quarter-dollar) with no impact on the public or on
stakeholders.
2. 80/20 matches the current material in both EMS and in piece weight, having a weight
that falls within legally accepted variances for the current material.

41

In testing, 80/20 was 100% accepted by all three coin acceptor manufacturers.

125

3. Initial testing of other, potentially seamless, leaner-copper alternatives shows
potential for further incremental material savings without presenting any color
changes or corrosion-resistance changes.
Co-Circulate Materials

4. Plated-steel materials are a viable option for the five-cent (further testing will
determine feasibility for the dime), and offer up to approximately $29M in savings
annually over current materials. However, plated-steel materials have increased risks
of fraud and counterfeit, and are used in low-value foreign coins, all of which make
the materials not feasible for use in the quarter-dollar. They also have a significantly
lower die life, which, if not mitigated (see #6, below), could increase production and
labor costs, and reduce the savings the materials might offer.
5. Stainless steel, while resistant to corrosion, has a hardness that can negatively impact
its coinability. Control of cold-rolling reduction and proper annealing of the right
grades demonstrated the ability to mitigate this factor, and improves the coinability of
stainless steel, warranting further testing and evaluation. (See attached Stainless
Feasibility Study and its Executive Summary in Section 8.)
Production Improvement

6. Adjusting the height of relief/crown on our current coin designs by a fixed percentage
introduced other issues, such as outer elements (e.g., the border) filling before inner
ones, or the flow of the material changing. It became clear that changes to the coin
features—including adjustments to the height of relief/crown, planchet profile,
smoothing of design, softening of the letters, and less-detailed images in general—
must be treated as a collective system. This system involves not only the items
mentioned here, but also matching planchet-die geometry, strike force, die
lubrication/coating/polishing, and other variables.
7. Striking of coins with an outer nickel layer (whether single-layer NPS or multilayer
MPPS) will require that circulating dies be polished (to provide a uniform and smooth
surface) and coated (to provide sufficient abrasion resistance). PVD coatings on U.S.Mint-manufactured dies demonstrated poor adherence to die surfaces (coating
delamination).
8. To accommodate the abrasive outer nickel plating on NPS and MPPS, coating and/or
replacement of parts that contact the planchet/coin will be required in production
126

equipment (conveyors, material handling, press feed/takeaway parts and coin
counters). This will reduce identified material savings by an estimated $6M 42 per
year. A similar accommodation will be required by all external coin processors and
handlers to address the increased wear associated with nickel surfaces.
9. Variability and Pre-production trials indicate planchet lubrication is a critical, but
not-yet-optimized variable impacting coining performance with alternative materials.
The application of Carboshield BTX to our current cupronickel-based material
significantly improved die life and effectively raised the bar for alternatives.
However, it took the Mint over three years to develop and implement this
lubricant/anti-tarnish material. The Mint will need to develop a similar development
process for alternative materials.
10. The inclusion of more than just nickel and copper in leaner-copper-based alloys
impacts hardness and more critically conductivity. This will require development of
the annealing practices and also slight changes to the coin designs’ relief/crown.
11. Test strikes with different material, die designs, and planchet upset profiles confirm
that collectively these factors need to be treated as a complete system when making
changes. Results seen from changing one variable cannot be interpreted as solely
related to that one factor. This means changes to die designs, planchet upset, and
material composition will require structured trials to gain a broader understanding
and effectively interpret results.
Terminated Materials

12. Testing of plated zinc alternatives (copper-plated zinc (CPZ) and tin-plated copperplated zinc (TPCPZ)) showed insufficient wear and durability properties for
consideration on heavier denominations than the current one-cent CPZ application.
Additionally, TPCPZ exhibited galvanic corrosion when copper and tin, two
dissimilar metals were exposed to the environment during wear, rendering this
construction unsuitable for U.S. coins.

42

According to Schuler, the manufacturer of the presses in the Mint.

127

6.2.

Recommendations for Further Study
1. Continue 80/20 Testing and Evaluation
a. Continue larger-scale testing of 80/20 and develop a final specification that can
be utilized by current and other strip suppliers.
b. Conduct feasibility, variability and pre-production testing on cladding 80/20 to
a copper core as an alternative for the clad denominations of dime, quarterdollar and half-dollar. Direct cost savings from this change would be limited,
but continuing to clad these coins with the same alloy used in the five-cent
would streamline material production.

2. Pursue seamless alloy development
Continue alloy development of other, potentially seamless, leaner-copper
alternatives to provide opportunity for additional incremental materials
savings without impacting coin acceptors and coin processors. Initial testing
indicates further opportunity for incremental material cost reductions with a
composition evolving over several progressive steps.
3. Continue stainless steel R&D
a. Continue larger-scale variability and pre-production testing on the two
stainless steel grades identified in the attached Stainless Feasibility Study.
b. Conduct testing and evaluation of monolithic stainless steel as a clad outer
layer as a co-circulate material. Engineering calculations indicate this
combination could exhibit a similar EMS to the current clad coins and enable
the copper core thickness to be reduced, providing incremental material
savings and a reduction in the use of the more-expensive and price-volatile
nickel. Its piece weight, however, would be lighter.
4. Explore production improvements
a. Investigate push-back blanking and determine if that is a technically feasible
and cost-effective production method that would enable elimination of
internal annealing on strip material (see attached Laser-Blanking Study).
b. Pursue more-structured test strikes on different coin materials, modified
design aspects, and upset profile configurations to increase the Mint’s
understanding of the overall coin manufacturing system. These results can be
utilized to improve production efficiencies on current coin materials and
provide for quicker evaluation of future materials. Results from structured
trials can be used to support predictive model development and reduce the
need for time-consuming iterative test strikes.
128

7. Bi-Metallic Coin Study
Concurrent Technologies Corporation (CTC) performed the study on bi-metallic coins, and
recommended against the proposal to make bi-metallic five cents from current one-cent
coins as the center and five-cent coins as the outer ring. CTC also determined that bimetallic construction would be advisable for coin denominations above the dollar. Below is
the Executive Summary.
7.1.

Executive Summary

The Mint sought to leverage CTC’s recent experience in the Alternative Metals Study to
identify and quantify many of the issues associated with material selection, supply,
production, manufacturing and public use of bi-metallic coins.
CTC provided a tabular database entitled “World Bi-Metallic Coins” that includes countries
where the bi-metallic coins are issued, along with their denomination, images of the obverse
and reverse (when available), materials of construction, total coin weight and coin
dimensional specifications (thickness and diameter of the outer ring and core), insidediameter-to-outside-diameter (ID/OD) ratio, approximate United States (U.S.) equivalent
monetary value, Web site for images and other details, and the country’s mint or government
Web site. A total of 194 countries (including the United States) populate the World BiMetallic Coins database. Of the 194 total countries surveyed, 92 countries have one or more
bi-metallic coins in their nation’s coin set. From the World Bi-Metallic Coins database, CTC
observed that the ID/OD ratio of bi-metallic coins throughout the world varied between a
minimum of 0.56 and a maximum of 0.78. A mean ID/OD ratio of 0.68 was found.
CTC also investigated the feasibility and estimated unit cost of creating a circulating bimetallic coin using the current one-cent coin/planchet as an insert to an outer ring made
from a current five-cent coin/planchet. Demonstration pieces were fabricated (i.e., not
struck) and provided to the United States Mint to illustrate the placement of an already
circulated one-cent coin/planchet inside an outer ring made from an already circulated fivecent coin/planchet. These demonstration pieces also illustrated the effects of using an ID/OD
ratio of 0.90 (full diameter of a one-cent coin) and 0.68 (world mean ID/OD ratio); the outer
rim of material was removed from the one-cent coin to achieve an ID/OD ratio of 0.68.
Estimated unit costs were calculated for each possible one-cent coin/planchet in a five-cent
coin/planchet scenario.

129

CTC investigated the feasibility and cost effectiveness of utilizing a bi-metallic coin for
circulating coin denominations other than the five-cent coin. Manufacturing equipment
needed to produce bi-metallic coinage and production changes necessary to support
producing a bi-metallic coin for the United States in circulating coin quantities was
documented. Factors considered in the selection of potential metal alloys included color,
electrical conductivity, tarnish and corrosion resistance, wear resistance, electrochemical
compatibility with other alloys, cost, mechanical properties, coefficient of thermal
expansion, recyclability and environmental impact. By their nature, bi-metallic coins
require metals of differing colors. Of the many alternative alloys considered, the majority of
those selected for further evaluation was either already being used or were similar to alloys
already being used in production of world circulating bi-metallic coins. This included
copper-nickel alloys, various brasses and stainless steels.
Hypothetical two- and five-dollar circulating coins were contemplated and several
constructions were evaluated. This investigation was motivated by the discovery that at least
six bi-metallic world circulating coins, whose value exceeds $2 U.S. dollars, are currently in
circulation throughout the world. The hypothetical two- and five-dollar United States coins
were assumed to be 28 millimeters (mm) and 29.2 mm in diameter and 2.45 mm and 2.75
mm in rim height, respectively. These diameters fall between those of the legacy one-dollar
and half-dollar coins. The thickness of these two hypothetical coins is greater than any
current U.S. coin, but is less than other coins, including the United Kingdom one-pound
coin, circulated throughout the world. These hypothetical bi-metallic coins could be
produced by the United States Mint for 0.22 to 0.27 $/coin, depending upon the materials
used in their construction. Additional development, beyond the engineering cost analysis
described here, must be completed prior to selecting any of these designs for production.
Changes to the size and construction of the half-dollar coin were contemplated. A bimetallic construction was evaluated having an inside diameter of 14.8 mm, an outside
diameter of 22.73 mm and a rim height of 2.31 mm. The core of this hypothetical half-dollar
coin was made of homogeneous 75Cu-25Ni cupronickel while the outer ring was made of
Nordic gold. The projected unit cost for this coin was 0.143 $/coin (using FY2014 metal cost
and FY2013 United States Mint indirect costs for the quarter-dollar coin). The unit cost to
produce legacy 75Cu-25Ni-clad copper half-dollar coins for circulation in FY2006—the last
year that circulating half-dollar coins were produced—was 0.1749 $/coin; the projected cost
to produce legacy 75Cu-25Ni-clad copper half-dollar coins for circulation in FY2014 was

130

0.19132 $/coin. Therefore, the hypothetical bi-metallic half-dollar circulating coin would
offer a 25 percent reduction in unit cost compared to the legacy construction.
CTC performed a regulatory analysis of the applicable environmental issues, including those
related to air pollutant emissions, solid and/or hazardous waste management, water use and
wastewater discharges. CTC did not undertake a formal National Environmental Policy Act
(NEPA) environmental assessment as that was beyond the scope of the current project.
Recyclability of individual metal components prior to assembly was considered for the
materials considered as potential bi-metallic coin candidates. Two methods of recycling bimetallic coins were considered: 1) separation of the two metal constituents into two unique
streams and 2) blending of both metal constituents into a single recycle stream.
Based upon the information gathered from each of the above factors, CTC offers the
following recommendations for consideration and implementation by the United States
Mint. Detailed descriptions of the study’s findings and conclusions can be found in the body
of the report.
•

A bi-metallic five-cent coin, utilizing any materials for coin construction, will need to
co-circulate with the existing homogeneous cupronickel five-cent coin. If all
materials in a newly introduced bi-metallic five-cent circulating coin are nonferromagnetic, then a one-time investment of $277M is required by the United States
coin stakeholder community to accept the new coin construction. However, if any of
the components are ferromagnetic, then a one-time investment of $532M to upgrade
or replace existing coin-acceptance equipment will be needed. If a bi-metallic fivecent coin of different weight than the legacy five-cent coin was introduced into
circulation, additional sorting and handling would be required by United States coin
and currency handlers; the cost associated with this additional handling was
estimated to be $3.75M per year.

•

Do not pursue concept of one-cent core in five-cent outer ring using either previously
circulated coins or unstruck planchets. Significant technical and cost issues have been
identified with this bi-metallic coin construction.
o Technical issues, which cannot be overcome and therefore preclude the use of
either previously circulated coins or unstruck planchets, include the following.


A full-diameter one-cent coin/planchet placed inside a five-cent
coin/planchet outer ring would yield an inside-to-outside diameter
ratio of 0.90, which is well beyond the ratio of all other known bimetallic coins in circulation throughout the world. An outer ring of
such narrow width will be subject to warping, denting, crushing and

131

other damage during normal handling operations. In addition,
maintaining stability during assembly and striking will be problematic
and options for locking mechanisms between the one-cent
coin/planchet core and five-cent coin/planchet outer ring will be
severely limited with such a narrow outer ring.


Use of a reduced-diameter, previously circulated one-cent
coin/planchet will expose the zinc core, which would quickly corrode
during normal handling and exposure to the environment. This will
lead to decreased coin life and public confusion.



A full-diameter five-cent coin will not fit into the striking press collar
unless the outside diameter of the five-cent coin is first reduced by
upsetting or machining. This adds another processing step to the
production of such bi-metallic coins.



The approximately 0.3-mm thickness mismatch between the one-cent
and five-cent coins/planchets violates a recommendation by the leading
supplier of bi-metallic coin presses to keep such thickness mismatches
to less than 0.1 mm. Thickness mismatches greater than 0.1 mm would
tend to wear unevenly, collect debris along the corner formed by the
thinner component at the junction of the two components, likely
induce stress concentrations in the striking dies thereby shortening
useful die life and potentially require larger acceptance windows in
automated coin-acceptance devices due to inconsistencies associated
with placement of the two components in the thickness direction.

•

The one-cent’s date of striking, Lincoln’s profile, the shield and “ONE
CENT” are clearly visible on those demonstration pieces based on the
use of a previously circulated one-cent coin. During striking of the
resulting bi-metallic five-cent coin, a “double strike” condition would
occur as the original images would appear behind the newly struck
image. Furthermore, the alignment of the two images would be
random leading to wide variations in the final struck image and
potentially leading to increased variability in finished coin quality.

o Introduction of such a bi-metallic five-cent coin into circulation, would not
offer the same amount of unit cost savings as other alternative five-cent coin
constructions as identified in the Alternative Metals Study. Furthermore,
additional sorting and handling of this construction, which would require cocirculation, would require an estimated increase of $3.75M/year by the coin
and currency handlers. Also, less expensive options consisting of
homogeneous non-ferromagnetic stainless steel construction were identified in
the Alternative Metals Study.
132

o An option to use a full-thickness copper-plated zinc core was considered. Of
the three constructions evaluated, only one provided any significant unit cost
savings. However, this construction relied on nickel-plated steel for the outer
ring resulting in a complex metal mixture that:


Is susceptible to rapid corrosion



Requires upgrades or replacements for many coin-acceptance devices
by domestic coin stakeholders at a cost of $532M since the associated
steel alloys are ferromagnetic



Requires additional sorting and handling by the coin and currency
handlers at an annual cost of $3.75M.

•

Consider use of a clad core for any bi-metallic coins with a face value greater than or
equal to one dollar to increase security and visual uniqueness. According to the
guidelines defined in the European Vending Association (EVA) Coin Design
Handbook, bi-metallic coins are suitable for higher-value coins, which are defined as
those whose value is approximately greater than 50 Euro cents (approximately 68
United States cents). Security features, such as clad core bi-metallic construction, are
highly recommended to deter counterfeits—the clad-core bi-metallic construction is
the highest security feature commonly available in circulating coins according to the
EVA Coin Design Handbook. The added cost for a clad core bi-metallic coin was
found to be between 0.02 and 0.03 $/coin more than a homogeneous core design.
Therefore, the added security offered by a clad core was judged to be worth the
additional cost for coins that typically can be produced in circulation quantities for
0.18 to 0.27 $/coin depending on material selection and coin dimensions.

•

Use an ID/OD ratio between 0.60 and 0.75 for bi-metallic coins. Maintaining this
ID/OD ratio is consistent with the majority of bi-metallic circulating coins in the
world. This ratio is consistent with a recommendation by the manufacturer of the
overwhelming majority of the world’s coin striking presses to keep the exposed areas
of the two components (i.e., the core and outer ring) approximately equal. Deviations
from equal areas sometimes occur to minimize the quantity of the more expensive of
the two components of a bi-metallic coin. The unit cost of bi-metallic coins did not
vary widely over an ID/OD ratio between 0.60 and 0.75 indicating that other factors,
including artistic appeal, may play an important role in selecting the desired ID/OD
ratio for any given bi-metallic coin.

•

Use a minimum outer ring width (i.e., the difference between the outside radius and
inside radius) of 4.0 mm. A leading coin striking press manufacturer recommends
that the width of the outer ring be a minimum of 3.5–4.5 mm to ensure that highquality outer rings are delivered to, and maintained during operations within, the bimetallic coining presses. A range in widths is given since the recommended value for

133

any given coin depends on the thickness and outside diameter of the outer ring; larger
widths apply to outer rings of larger diameter.
•

Prior to introducing any circulating coin of new construction, including bi-metallic
construction, engage the coin-acceptor community to test for uniqueness from other
circulating coins used throughout the world. The United States Mint should provide
manufacturers of automated coin-processing equipment samples of the final coins
(made from the new materials of construction) at least 18 months in advance of the
expected date for introducing these coins into circulation. Doing so will provide the
coin-processing industry time to respond to changes in the construction of coins.
These samples are expected to be used to design the necessary changes to the
manufacturer’s equipment and to get their clients prepared for the introduction of
these coins into circulation.

•

Within the sizes of the current United States coin set, use of piercings from highdenomination bi-metallic coins is not practical for low-value coins of smaller
diameter. In no cases were the thickness and diameter of such piercings (within the
bounds of acceptable ID/OD ratios for bi-metallic coins) acceptable for striking. In all
cases, the piercing size violated the thickness and diameter tolerances required of
planchets used to produce these low-denomination coins.

•

The capital cost required by the United States Mint to produce bi-metallic coins
would increase the unit cost of coins by approximately 0.0066 $/coin. This assumes
the use of piercing presses, new vertical coin striking presses, additional upsetting
mills and inspection of outer rings. A 10-year return on investment was used for this
calculation.

Production of bi-metallic coins at the United States Mint will require additional process steps
and production equipment compared to the legacy coin production. Compared to the
production of homogeneous or clad coins, bi-metallic coins require the following additional
processing steps: one additional blanking operation, one additional upsetting operation, a
piercing operation and inspection of the outer ring. Two options exist for production of bimetallic coins: 1) processing of materials from rolled coils to finished bi-metallic coins at the
United States Mint and 2) striking pre-assembled bi-metallic planchets produced by a
supplier. Both options will require purchase of additional vertical presses and support
equipment; a similar number of additional vertical presses and support equipment would be
required for either option to meet the production demands of the United States Mint. In the
first option, the United States Mint would purchase the equipment directly; in the second
option, the bi-metallic planchet supplier would purchase the equipment (and indirectly pass
the cost onto the United States Mint). In the first option, the United States Mint could retire
their current horizontal striking presses (or use them for production of non-bi-metallic

134

coins). However, if the second of these options is exercised, then the United States Mint
must still use its existing horizontal striking presses to strike the bi-metallic pre-assembled
planchets. In effect, an additional, and costly processing step will be required for this option:
the assembled components must be compressed with a flat die to lock them together and to
ensure they remain intact during subsequent handling, shipping and loading into the
horizontal striking presses at the United States Mint. As a result, CTC expects the cost
impact to the United States Mint for this second production option to be higher than having
the United States Mint complete all production steps in-house.

135

This page intentionally left blank.

136

8. Stainless Steel Feasibility Study
Concurrent Technologies Corporation (CTC) performed the study on Stainless Steel
alternatives, and published that report to the Mint in early July 2014. Below is the Executive
Summary, formatted for this report.
8.1.

Executive Summary

The United States Mint sought to leverage CTC’s recent experience in the Alternative Metals

Study and CTC’s broad understanding of metals, manufacturing and coin production to
identify and quantify many of the issues associated with material selection, supply,
production, manufacturing and public use of stainless steel coins. Key to the success of the
current effort was the willingness of the suppliers to provide laboratory heats (each weighing
approximately 50 pounds) of down selected stainless steel alloys for evaluation. Stainless
steel alloys having low hardness, strength and work hardening behavior, while achieving
complete die fill and the ability to upset blanks in a softened, annealed state to minimize
striking loads and die fatigue, were down selected for this project. The results of this study
include the following.
•

•
•

•

•

A material change from cupronickel to a stainless steel alloy for the existing five-cent
coin would require co-circulation (although non-seamless) with the legacy coin; nonseamless alternative candidates having a different, possibly unique, EMS and/or a
different weight than the incumbent coinage.
Stainless steel alloys would provide a lower-cost candidate for the five-cent
circulating coin.
Based upon the United-States-Mint-approved cost analysis methodology used, all
stainless steel alloys evaluated offer a unit cost saving to the United States Mint for
five-cent circulating coins.
While the unit cost saving to the United States Mint for ferromagnetic alloys were
found to be higher than that for non-ferromagnetic alloys, use of ferromagnetic
stainless steel coins would have approximately twice the cost impact to the domestic
coin stakeholders (including the vending industry, laundromats and others) than
would the use of non-ferromagnetic stainless steel coins.
Rittenhouse and Modified 18-9 LW appeared to offer good striking performance at
striking loads that were comparable to those used to manufacture the legacy
cupronickel five-cent circulating coins. However, validation of production
parameters using production equipment (as opposed to the laboratory-scale heats and
equipment evaluated and discussed in this report) at the suppliers need to be

137

evaluated; therefore, larger scale tests are recommended before attempting a
preproduction run.
Based upon these findings, the following recommendations are offered.
•

•
•

•

Complete additional technical assessments of Rittenhouse 52 and Modified 18-9 LW
stainless steel alloys. Striking of these alloys during tests completed at the United
States Mint Research and Development Center in Philadelphia showed complete die
fill with reduced coining loads as compared to the incumbent cupronickel five-cent
circulating coin.
Consider only non-ferromagnetic stainless steel alloys for use in five-cent coins to
minimize the impact to the domestic coin stakeholders.
Confirm unit cost estimates by obtaining updated cost quotes from material vendors
for production volumes of stainless steel five-cent coins and completing
preproduction runs to validate striking die life.
Apply numerical methods (such as finite element analysis) to predict blanking shear
stresses, die fill, die stress and die life for various materials, die shape and process
conditions. Doing so will improve the understanding of how these factors interact in
advance of actual pre-production trials. The virtual trials will allow for relatively
inexpensive investigations of many process design scenarios, which will enhance the
probability of achieving successful and meaningful pre-production trials.

138

9. Laser-Blanking Study
Fraunhofer USA performed the study on laser blanking, and published that report to the
Mint in July 2014. Below is the Executive Summary, formatted for this report.
9.1.

Executive Summary
In support of the Coin Modernization, Oversight, and Continuity Act of 2010, the
U.S. Mint is seeking ways to reduce the cost of producing circulating coins. One
potential idea is to replace the current mechanical die blanking and on-site annealing
with laser blanking and off-site bulk annealing. A second scenario is to retain the onsite annealing and exchange die-blanking with laser blanking. The U.S. Mint
contracted with Fraunhofer USA to investigate the technical and financial feasibility
of these ideas.
Fraunhofer conducted a thorough review of the technical issues and found no
significant concerns. The review involved laser cutting nine different materials and
making sample coin blanks. The sample blanks were characterized for diameter, burr,
knit-line, edge condition, grain structure, and hardness in the area adjacent to the
laser cutting. Laser cutting of the monolithic 5-cent material was found to be faster

and at better edge quality than with any of the clad materials (dime, quarter, and
dollar). Sample lots of 100 pieces of 5-cent, dime, quarter, and dollar blanks were sent
to the U.S. Mint for evaluation.
A conceptual design was developed along with 3D CAD images showing how
multiple lasers working in parallel could meet the production needs of the U.S. Mint.
Also an Environmental Assessment was performed which yielded no significant
concerns.
Several economic analyses were performed using a range of assumptions and none of
the analyses showed a strongly favorable economic outcome for laser blanking. When
considering laser blanking machines with production capacity equal to the current die
blanking machines, laser blanking looks economically unfavorable. When lower
production capacity was considered, the economics of laser blanking are roughly
equivalent to die blanking within the margin of error of the analysis, making laser
blanking not a very compelling avenue for pursuing cost reduction efforts. Perhaps in

139

the future, if lasers cut faster or become less expensive, that situation might change;
but currently the financial feasibility of laser blanking looks challenging.
In the course of this study, Fraunhofer identified a promising alternative to laser
blanking called die blanking with a push-back system, which could eliminate the
expense of on-site annealing. This system is very similar to the current die blanking
and the capital investment looks to be low. Fraunhofer recommends that a study be
conducted of a push-back die blanking system for the U.S. Mint.
If the U.S. Mint decides that a lower production capacity meets its needs, then the
economics of laser blanking are estimated to be roughly equal with die blanking and
laser blanking might be pursued by the U.S. Mint for some of the benefits it offers.
Fraunhofer has developed a logical multiphase development process to continue the
effort into laser blanking that will address some of the design and production
questions while minimizing development expenses.
Circulating coins are manufactured with three successive metal forming steps. 1) Punch out a
flat circular disk, called a blank, from a flattened coil of “hard” sheet metal. 2) Raise a ridge
along the outer circumference of the blank (known as upsetting the blank) to create what is
known as a planchet. 3) Coin the planchet by stamping the top and bottom surfaces with
artwork such as the faces of U.S. Presidents and required inscriptions associated with U.S.
coinage. The first step in this sequence, blanking, is the subject of the current cost reduction
effort.
Mechanical die blanking is a simple process that works like a paper hole-punch with the
punch positioned above the sheet metal and the die below. The die sets are constructed with
multiple punches so that each time the die closes, as many as 20 blanks are created. The die
press runs at 550 strokes per minute which means that over 5 million blanks can be produced
in a single 8 hour shift.
In order to punch out a clean flat blank, the coils of sheet metal must be in a so called workhardened state rather than a soft, or annealed, state. Unfortunately, the final metal forming
step (stamping) requires the metal to be in an annealed state. This means that the U.S. Mint
must run large and expensive rotary retort furnaces to anneal all the coin blanks on site.
The proposed laser blanking process, however, is capable of directly cutting annealed sheet
material. Thus if laser blanking is technically and financially feasible, it would be possible to

140

eliminate the rotary retort furnaces at the U.S. Mint facilities. The responsibility of
annealing the coiled sheet metal material would then be shifted to the metal suppliers who
are believed to be able to anneal the metal in bulk coil form at a lower cost compared to the
U.S. Mint’s rotary retort furnaces.
The work performed by Fraunhofer was structured into four areas
1)
2)
3)
4)

Technical feasibility
Conceptual design
Environmental assessment
Economic feasibility

Technical feasibility was performed by cutting out sample blanks using a 6KW Trumpf laser
and quantifying the quality of the resulting blanks. In total, nine different materials were
cut. Naturally the five existing coin materials were cut, 5-cent 43, Dime, Quarter, Half-Dollar,
and Dollar (note that the penny was not tested because it is not blanked at the U.S. Mint).
Also, four possible future alternative materials were cut: 304 stainless steel, 430 stainless
steel, brass, and silicon steel.
Once the samples were cut, various pieces of metrological equipment were used to quantify
six different areas of concern: 1) diameter, 2) burr, 3) edge condition (chamfer), 4) knit-line,
5) grain structure, and 6) hardness in the heat affected zone (HAZ).
The diameter data raised no concerns since the blank diameter is easily adjusted in the
machine and the range of diameters (sample to sample variation) was within acceptable
limits, less than ±0.002” (±50µm). Some samples were found to be excessively elliptical, a
problem that was mostly resolved with improved sample fixturing and would likely be
completely resolved by switching to a rotary actuator from the X-Y actuator used in the test
setup.
The edge burrs raised no concerns as they were typically around 0.001” (25µm) or less once
the laser process parameters were optimized.

The word “nickel” is ambiguous as it can mean either a five cent coin or a silver metallic material. Both the
coin and the metal are discussed in this document leading to possible confusion. To reduce the chance of
confusion, the term “five-cent” is used in this document to refer to the coin whereas “nickel” is used in
reference to the metal.

43

141

The edge condition (chamfers) of some of the laser cut blanks raised some initial concerns
but ultimately the chamfers were deemed acceptable. Edge chamfers on some of the clad
copper blanks (e.g. quarters) were as large as 0.004” (100µm), which raised the initial
concerns. However, two additional studies removed the concerns. Firstly, die blanked
samples (the current process) were found to have edge chamfers of a similar size (particularly
on the quarter blanks). Secondly, a set of die-cut 5-cent blanks were modified to have
0.002”, 0.004”, and 0.008” chamfers (50, 100, and 200µm) and then processed into coins at the
U.S. Mint. The samples were found to produce acceptable coins even with as much as 0.008”
(200µm) chamfer on one edge.
Knit-line is a term chosen to describe a small bump at the edge of the coin blank at the
location where the laser starts and stops cutting. This bump can be as large as 0.008”
(200µm) and is a concern because it could cause problems in feeding the blanks into the
upsetting machine or in actually upsetting the blanks. If the knit-line does cause a problem,
Fraunhofer is confident that a laser cutting machine could be designed to hold the blank
while it is being cut which would eliminate the knit-line.
Grain structure within the HAZ did not raise any concern. Prior to testing, there were
concerns that the heat from the laser would create edge hardening which might make
upsetting or stamping difficult with laser cut blanks. However, the only observable change
was some signs of grain growth when hard samples were cut which indicates the material is
softening rather than hardening.
Hardness measurements did not raise any concern, with one exception. When hard samples
were laser cut, the material hardness frequently decreased, which is not a concern. When
annealed samples were laser-cut, no change in hardness was measured. One exception was
304 stainless steel which showed a significant increase in hardness in the HAZ which might
cause difficulties when trying to upset blanks or stamp planchets made from that material.
The hardness at the edge of the laser cut 304 blanks increased to 250 (HV100) which is about
twice as hard as the current, annealed cupronickel materials being processed at the Mint. A
previous alternative metals study performed for the U.S. Mint showed this material was
difficult to strike due to its hardness, so any increase in hardness would only make this
situation worse.
Overall, laser cutting of blanks appears to be technically feasible. Some careful engineering
design might be needed for the laser blanking machine, but no fundamental problems with
laser cutting were identified.
142

While producing high quality laser cut blanks was shown to be possible, it was known that
they would need to be cut very quickly. The current mechanical die blanking system cuts
metal at the equivalent of 600 linear meters per minute. Testing with the lasers showed that
the cutting speed for current coin materials is between 14 and 35 meters per minute. To
have a laser machine match the performance of the die blanking machine would require a
machine design with multiple lasers, and immediately raised concerns about the cost of the
machine.
In order to make an estimate of the cost of laser blanking, it was necessary to have a
conceptual design of a laser blanking machine. The overall concept is to have multiple lasers
cutting blanks at the same time to improve the throughput of the machine. A number of
lasers (perhaps 4) would be mounted side by side across the width of the strip. These lasers
would each be mounted on rotary stages that would move in a circular motion. The stages
would be actuated with individual actuators or, as a secondary option, with a mechanism
that drives them together as a group. The group of stages would also be mounted on a stage
that allowed the laser cutting to start (the pierce) slightly to the side of the coin blank.
Additional groups of lasers (perhaps 4 rows of 4 lasers, total 16) would be located
downstream of the first group to cut more blanks. This layout is actually similar to the
punch and die positions in the current blanking machine, although the lasers would likely
need more space than punches and dies.
The footprint of the laser machine would be more than the current die-blanking press, but
significantly less than the space made available by the elimination of the rotary retort
furnace. If the rotary retort furnace is retained, Fraunhofer believes the laser blanking
system could still be made to fit within the current footprint, but the engineering design
would be more difficult. A laser blanking machine requires a significant amount of support
equipment including the lasers themselves, chillers, air handlers, and nitrogen generators
which will consume significant floor area. It is recommended that a mezzanine be
constructed above the laser cutting machine to hold the various pieces of support equipment.
The laser blanking system (with mezzanine) should easily fit within the available floor space
of the U.S. Mint. Lower ceiling heights in Denver might require an alternative placement of
support equipment.
The environmental assessment raised no concerns. Eliminating the annealing furnaces at the
U.S. Mint would eliminate potential sources of both air and water pollution (though neither
are really a serious concern as they are carefully managed by the U.S. Mint). Laser cutting

143

will use additional electricity and the bulk annealing at the suppliers might shift
environmental concerns from the U.S. Mint facility to supplier locations, but there is no
significant cause for concern.
The financial feasibility study, however, cast significant doubt about the proposed savings
from the laser based blanking system. On the positive side, laser blanking of 5-cent coins
might be slightly less expensive than the current die blanking owing to the relatively high
speed cutting that is possible on the cupro-nickel material that the 5-cent is made from. On
the negative side, the slower laser cutting on the clad copper materials (dime, quarter, halfdollar, and dollar) make laser cutting significantly more expensive than the current die
blanking. Slower cutting means that more lasers working in parallel are needed, increasing
both the cost of the machine and the electricity to run it and also the cost of consumables
(e.g. filters). Furthermore, designing a machine that would potentially require over 30 lasers
would be a challenge. Fraunhofer is aware of commercial laser cutting machines with 2
lasers, but no more than that. But it is worth noting that current commercial machines are
sold based on their flexibility, whereas the U.S. Mint does not need geometric flexibility
which greatly simplifies the design and control of multiple lasers.
The economic analysis that looked most favorable for laser blanking was replacing all ten
production lines with laser blanking machines with lower production capacity, either halfspeed or annealing speed 44. For this analysis, the economics of laser and die blanking were
roughly equal, at least within the uncertainty of the analysis. This analysis could be used as
justification to further pursue laser blanking, however, the switch to laser blanking does not
look to be a promising venue for significant cost savings and carries some development risks.
One of the key findings from the economic analyses is that the savings from off-site bulk
annealing of the coin material proved to be less than expected. This meant that it was not as
easy to use the savings from the annealing costs to help cover the cost of laser blanking.
Given that laser blanking appears to be technically feasible but financially uncompelling,
there are a few options that can be considered:
1) Take no further action.
A half speed machine is one that has a production capacity of half the current die blanking machine. An
annealing speed machine has a production capacity that is equal to the current annealing furnace production
capacity. Both are capable of delivering FY2013 production volumes, despite having lower production capacity.
44

144

2) Undertake a prototype development effort to make a single laser blanking machine to
address issues such as knit-line, rotary stage cutting, and practical cutting speeds.
Experience gained from the prototype development would decrease the risks
associated with laser blanking, decrease economic uncertainty, and allow the U.S.
Mint to gain valuable experience with this new blanking technology.
3) Undertake a study of non-laser based blanking alternatives such as die-blanking with
a push-back station that might be able to directly blank annealed material without
distorting the blanks.
4) Undertake a study of waterjet cutting blanks.
It is Fraunhofer’s recommendation to proceed with option 3 and possibly option 2 above.
Die-blanking with a push-back station is viewed as a strong candidate for cost-reducing the
blanking operation at the U.S. Mint and laser blanking might be useful as well, although the
current analysis suggests it is likely not a strong candidate. Waterjet cutting is believed to be
slow and somewhat messy and not likely to be a good fit for the U.S. Mint’s application.

145

This page intentionally left blank.

146

10.Appendices
10.1.

Wear Test Results – Variability Lots

10.1.1.Copper-Plated Zinc (CPZ)

147

10.1.2.Tin-Plated CPZ (TPCPZ)

TPCPZ Five-Cent (Variability)

148

TPCPZ Quarter-Dollar (Variability)

149

10.1.3.NPS

NPS Five-Cent (Variability)

150

NPS Quarter-Dollar (Variability)

151

10.1.4.MPPS

MPPS Five-Cent (Variability)

152

MPPS Quarter-Dollar (Variability)

153

10.1.5.80/20A (Variability)

154

10.1.6.80/20B (Variability)

155

10.2.

Steam Test Results – Variability Lots

10.2.1.CPZ Steam Test

156

10.2.2.TPCPZ Steam Test

TPCPZ (Five-Cent) (Variability)

157

TPCPZ (Quarter-Dollar) (Variability)

158

10.2.3.NPS Steam Test

NPS Five-Cent (Variability)

159

NPS Quarter-Dollar (Variability)

160

10.2.4.MPPS Steam Test

MPPS Five-Cent (Variability)

161

MPPS Quarter-Dollar (Variability)

162

10.2.5.80/20A Steam Test (Variability)

163

10.2.6.80/20B Steam Test (Variability)

164

10.3.

Conductivity and CSV Test Results – Variability Lots

10.3.1.CPZ Conductivity and CSV

Conductivity – Nominal CPZ (Variability)

Electrical Conductivity (% IACS)

Page
_1_of_1__

Date: 4-Feb-14
Conductivity Sigma Test D 2.068 Foerster (Cert: 20130200Meter: 51386) Due March 25, 2014
Operator: Barry Claybrook
Material: CPZ 5c Nominal Plating
Form: Planchets (10 Kg)

FREQUENCY
1
2
3
4
5
6
7
8
9
10
11
12
13
14
15
16
17
18
19
20

1 = ___60__kHz
28.47
28.41
28.43
28.380
28.47
28.410
28.36
28.43
28.450
28.45
28.48
28.47
28.450
28.47
28.5
28.47
28.47
28.48
28.4
28.450

2 = __120__kHz
28.62
28.64
28.53
28.64
28.62
28.590
28.59
28.55
28.66
28.64
28.69
28.64
28.660
28.66
28.67
28.69
28.72
28.66
28.62
28.640

3 = __240__kHz
28.93
28.930
28.97
28.930
28.91
28.970
28.86
28.88
28.97
28.91
28.95
29
28.910
29
28.95
29.02
28.78
28.86
28.97
28.900

4 = __480__kHz
29.21
29.28
29.34
29.22
29.24
29.22
29.31
29.24
29.26
29.47
29.36
29.26
29.19
29.47
29.36
29.55
29.33
29.20
29.34
29.34

Average
Median
SD
Min
Max

28.45
28.45
0.037
28.36
28.50

28.64
28.64
0.046
28.53
28.72

28.93
28.93
0.057
28.78
29.02

29.31
29.30
0.099
29.19
29.55

165

Conductivity – Min CPZ (Variability)

Electrical Conductivity (% IACS)

Page
_1_of_1__

Date: 4-Feb-14
Conductivity Sigma Test D 2.068 Foerster (Cert: 20130200Meter: 51386) Due March 25, 2014
Operator: Barry Claybrook
Material: CPZ 5c Minimum Plating
Form: Planchets (10 Kg)

FREQUENCY
1 = _____60__kHz

2 = ____120__kHz

3 = ____240__kHz

4 = ___480__kHz

1

28.17

28.22

28.53

28.83

2

28.02

28.22

28.450

28.79

3

28.12

28.29

28.48

28.79

4

28.000

28.21

28.500

28.76

5

28.12

28.26

25.5

28.84

6

28.120

28.240

28.520

28.86

7

28.12

28.31

28.53

28.72

8

28.22

28.22

28.57

28.76

9

28.170

28.28

28.57

28.84

10

28.12

28,28

28.56

28.78

11

28.21

28.24

28.5

28.76

12

28.21

28.31

28.53

28.74

Average

28.13

28.25

28.25

28.79

Median

28.12

28.24

28.52

28.79

SD

0.069

0.034

0.912

0.044

Min

28

28.21

25.5

28.72

Max

28.22

28.31

28.57

28.86

166

CSV –Planchet CPZ (Variability)

CSV – Coin CPZ (Variability)

167

10.3.2.TPCPZ Conductivity and CSV

Conductivity – Max TPCPZ (Five-Cent) (Variability)

Electrical Conductivity (% IACS)
Date:
Conductivity
Meter:
Operator:
Material:
Form:

4-Feb-14
Sigma Test D 2.068 Foerster (Cert: 2013020051386) Due March 25, 2014
Barry Claybrook
TPCPZ 5c Horizontal Max Plating
Planchets (10 Kg)

1=
_____60__kHz

1
2
3
4
5
6
7
8
9
10
11
Average
Median
SD
Min
Max

Page
_1_of_1__

FREQUENCY

2=
____120__kHz

3=
____240__kHz

4 = ___480__kHz

28.53
28.55
28.59
28.6
28.53
28.62
28.55
28.5
28.53
28.62

30.57
30.38
30.4
30.64
30.38
30.53
30.31
30.71
30.55
30.43

28.56
28.55
0.042
28.5
28.62

30.49
30.48
0.129
30.31
30.71

168

Conductivity – Max TPCPZ (Quarter-Dollar) (Variability)

Electrical Conductivity (% IACS)

Page
_1_of_1__

Date: 4-Feb-14
Conductivity Sigma Test D 2.068 Foerster (Cert: 20130200Meter: 51386) Due March 25, 2014
Operator: Barry Claybrook
Material: TPCPZ 25c Horizontal Max Plating
Form: Planchets (10 Kg)

FREQUENCY
1=
_____60__kHz

2=
____120__kHz

3=
____240__kHz

4 = ___480__kHz

1
2
3
4
5
6
7
8
9
10
11
12

28.57
28.79
28.71
28.9
28.81
28.84
28.86
28.81
28.74
28.88
28.86

30.66
30.6
30.78
30.72
30.38
30.64
30.41
30.64
30.57
30.6
30.64

Average
Median
SD
Min
Max

28.80
28.81
0.095
28.57
28.90

30.60
30.64
0.119
30.38
30.78

169

Conductivity – Nominal TPCPZ (Five-Cent) (Variability)

Electrical Conductivity (% IACS)
Date:
Conductivity
Meter:
Operator:
Material:
Form:

4-Feb-14
Sigma Test D 2.068 Foerster (Cert: 2013020051386) Due March 25, 2014
Barry Claybrook
TPCPZ 5c Oblique Nom Plating
Planchets (10 Kg)

Page
_1_of_1__

FREQUENCY
1=
_____60__kHz

1
2
3
4
5
6
7
8
9
10
11
12
Average
Median
SD
Min
Max

2=
____120__kHz

3=
____240__kHz

4 = ___480__kHz

28.48
28.57
28.53
28.52
28.57
28.59
28.55
28.53
28.55
28.57
28.59

30.48
30.4
30.62
30.53
30.76
30.97
30.379
30.78
30.79
30.76
30.57

28.55
28.55
0.033
28.48
28.59

30.64
30.62
0.187
30.379
30.97

170

Conductivity – Nominal TPCPZ (Quarter-Dollar) (Variability)

Electrical Conductivity (% IACS)

Page
_1_of_1__

Date: 4-Feb-14
Conductivity Sigma Test D 2.068 Foerster (Cert: 20130200Meter: 51386) Due March 25, 2014
Operator: Barry Claybrook
Material: TPCPZ 25c Oblique Nom Plating
Form: Planchets (10 Kg)

FREQUENCY
1=
_____60__kHz

2=
____120__kHz

3=
____240__kHz

4 = ___480__kHz

1
2
3
4
5
6
7
8
9
10
11
12

28.66
28.6
28.57
28.62
28.66
28.72
28.62
28.69
28.66
28.76
28.71

29.88
30.41
30.12
30.07
30.21
30.41
30.22
30.17
30.33
30.29
30.31

Average
Median
SD
Min
Max

28.66
28.66
0.056
28.57
28.76

30.22
30.22
0.157
29.88
30.41

171

Conductivity – Min TPCPZ (Five-Cent) (Variability)

Electrical Conductivity (% IACS)

Page
_1_of_1__

Date: 4-Feb-14
Conductivity Sigma Test D 2.068 Foerster (Cert: 20130200Meter: 51386) Due March 25, 2014
Operator: Barry Claybrook
Material: TPCPZ 5c Horizontal/Oblique Min Plating
Form: Planchets (10 Kg)

FREQUENCY
1 = _____60__kHz

2 = ____120__kHz

3 = ____240__kHz

4 = ___480__kHz

1

28.19

29.22

2

28.4

29.12

3

28.38

29.02

4

28.24

29.17

5

28.21

29.12

6

28.38

29.38

7

28.38

29.09

8

28.28

29.14

9

28.34

29.07

10

28.36

29.16

11

28.38

28.98

12

28.33

29.22

13

28.29

29.1

14

28.33

29.22

15

28.36

29.31

16

28.29

29.19

17

28.33

29.1

18

28.34

29.31

19

28.33

29.38

20

28.31

29.4

28.28

29.31

Average

28.32

29.13

Median

28.36

29.12

SD

0.077

0.106

Min

28.19

28.98

Max

28.40

29.40

172

Conductivity – Min TPCPZ (Quarter-Dollar) (Variability)

Electrical Conductivity (% IACS)

Page
_1_of_1__

Date: 4-Feb-14
Conductivity Sigma Test D 2.068 Foerster (Cert: 20130200Meter: 51386) Due March 25, 2014
Operator: Barry Claybrook
Material: TPCPZ 25c Horizontal/Oblique Min Plating
Form: Planchets (10 Kg)

FREQUENCY
1=
_____60__kHz

2=
____120__kHz

3=
____240__kHz

4 = ___480__kHz

1
2
3
4
5
6
7
8
9
10
11
12

28.48
28.52
28.62
28.55
28.53
28.59
28.52
28.55
28.6
28.64
28.62

29.26
29.22
29.09
29.03
29.14
29.16
29.17
29.34
29.12
29.33
29.38

Average
Median
SD
Min
Max

28.57
28.55
0.051
28.48
28.64

29.20
29.17
0.112
29.03
29.38

173

CSV – Planchet TPCPZ (Five-Cent) (Variability)

CSV – Planchet TPCPZ (Quarter-Dollar) (Variability)

174

CSV – Coin TPCPZ (Five-Cent) (Variability)

CSV – Coin TPCPZ (Quarter-Dollar) (Variability)

175

10.3.3.NPS (Conductivity Test Not Applicable)

CSV – Planchet NPS (Five-Cent) (Variability)

CSV – Planchet NPS (Quarter-Dollar) (Variability)

176

CSV – Coin NPS (Five-Cent) (Variability)

CSV – Coin NPS (Quarter-Dollar) (Variability)

177

10.3.4.MPPS (Conductivity Test Not Applicable)

CSV – Planchet MPPS (Five-Cent) (Variability)

CSV – Planchet MPPS (Quarter-Dollar) (Variability)

178

CSV – Coin MPPS (Five-Cent) (Variability)

CSV – Coin MPPS (Quarter-Dollar) (Variability)

179

10.3.5.80/20A (Conductivity Results Unavailable)

CSV – Planchet 80/20A (Variability)

CSV – Coin 80/20A (Variability)

180

10.3.6.80/20B (Conductivity Results Unavailable)

CSV – Planchet 80/20B (Variability)

CSV – Coin 80/20B (Variability)

181

10.4.

Wear Test Results – Pre-Production

10.4.1.NPS

NPS Pilot Material (Five-Cent)

182

NPS Pilot Material (Quarter-Dollar)

183

NPS Pre-production (Five-Cent)

184

NPS Pre-production (Quarter-Dollar)

185

10.4.2.MPPS

MPPS (Five-Cent) (Pre-Production)

186

MPPS (Quarter-Dollar) (Pre-Production)

187

10.4.3.80/20B

Initial 80/20B Five-Cent (Pre-Production)

188

Treated 80/20B Five-Cent (Pre-Production)

189

10.4.4.CPZ

CPZ Five-Cent (Pre-Production)

190

10.5.

Steam Test Results – Pre-Production

10.5.1.Nickel-Plated Steel

NPS Pilot Material (Five-Cent)

191

NPS Pilot Material (Quarter-Dollar)

192

NPS Pre-production (Five-Cent)

193

NPS Pre-production (Quarter-Dollar)

194

10.5.2.MPPS

MPPS (Five-Cent) (Pre-production)

195

MPPS (Quarter-Dollar) (Pre-production)

196

10.5.3.80/20B

80/20B Five-Cent (Pre-Production)

197

80/20B Five-Cent Lubricated (Pre-Production)

198

10.5.4.CPZ

CPZ Five-Cent (Pre-Production)

199

10.6.

CSV Test Results – Pre-Production

10.6.1.NPS

NPS Pilot Material – Planchet (Five-Cent)

NPS Pilot Material – Planchet (Quarter-Dollar)

200

NPS Pilot Material – Coin (Five-Cent)

NPS Pilot Material – Coin (Quarter-Dollar)

201

NPS Pre-production – Planchet (Five-Cent)

NPS Pre-production – Planchet (Quarter-Dollar)

202

NPS Pre-production – Coin (Five-Cent)

NPS Pre-production – Coin (Quarter-Dollar)

203

10.6.2.MPPS

MPPS Pre-production – Planchet (Five-Cent)

MPPS Pre-production – Planchet (Quarter-Dollar)

204

MPPS Pre-production – Coin (Five-Cent)

MPPS Pre-production – Coin (Quarter-Dollar)

205

10.6.3.80/20B

80/20B Pre-production – Planchet (Five-Cent)

80/20B Pre-production – Coin (Five-Cent)

206

10.6.4.CPZ

CPZ Pre-production – Planchet (Five-Cent)

CPZ Pre-production – Coin (Five-Cent)

207

10.7.

CSV Comparison—Plated Steel v. Current Material

MATERIAL
(Five-Cent))

CSV ELECTROMAGNETIC SIGNATURES
AVERAGE / RANGE WIDTH

COMMENTS

Inner
Conductivity 1

Inner
Conductivity 2

Inner
Permeability

Outer
Conductivity 1

Outer
Conductivity 2

Outer
Permeability

Current Cu-Ni

82 / 9.7

71 / 9.8

1004 / 14.5

70 / 3.4

75 / 3.4

1003 / 13.9

Current

80/20

84 / 9.6

73 / 9.4

1007 / 12.2

71 / 2.9

76 / 2.7

1007 / 10.1

Seamless

MPPS

91 / 35.8

99 / 44.9

485 / 24.4

70 / 9.9

91 / 10.2

501 / 20.9

NPS

68 / 32.5

76 / 43.5

472 / 27.8

62 / 8.8

85 / 8.6

488 / 20.9

Stainless (302HQ)

31 / 6.0

11 / 5.5

997 / 12.4

47 / 3.0

56 / 3.0

995 / 11.6

The first number is the average for that material. The second number is how much variance is seen in that material. The larger the second number, the wider the coin
acceptor’s “window” of acceptance must open to accept both.

MATERIAL
(Quarter-Dollar)

CSV ELECTROMAGNETIC SIGNATURES
AVERAGE / RANGE WIDTH

COMMENTS

Inner
Conductivity 1

Inner
Conductivity 2

Inner
Permeability

Outer
Conductivity 1

Outer
Conductivity 2

Outer
Permeability

Current Cu-Ni Clad

68 / 18.9

550 / 62.5

825 / 21.0

115 / 12.9

287 / 7.2

1006 / 15.5

Current

MPPS

176 / 44.9

189 / 60.7

400 / 17.5

113 / 16.5

131 / 18.1

475 / 37.2

Not Feasible

NPS

82 / 23.3

90 / 36.6

398 / 16.5

72 / 9.1

95 / 11.4

457 / 49.4

Not Feasible

1.

EMS ranges that overlap those of the current are highlighted in yellow.

2.

Plated-steel EMS ranges are wider than those of the current, necessitating wider acceptance windows and less security.

3.

Plated-steel and monolithic EMS ranges tend to overlap at multiple frequencies, diminishing the enhanced security of dual-frequency coin
validation.

4.

Cupronickel clad construction offers high security, as evidence by the low incidence of EMS overlap with MPPS and NPS.

208

11. Acronym List
°C

degrees Celsius

µm

micrometer, micron, 1 millionth of a meter

COGS

cost of goods sold

CPZ

copper-plated zinc

CSV

coin sorter/validator

DOE

Department of Energy

EMS

electromagnetic signature

EVA

European Vending Association

FRB

Federal Reserve Bank

IA

interagency agreement

IACS

International Annealed Copper Standard

IPR

independent peer review

IV&V

independent verification and validation

MPPS

multi-ply-plated steel

NIST

National Institute of Standards and Technology

NPS

nickel-plated steel

PL

public law

PVD

physical vapor deposition

R&D

research and development

RCM

Royal Canadian Mint

RM

The Royal Mint (UK)

SOP

standard operating procedures

TPCPZ

tin-plated, copper-plated zinc

USPS

United States Postal Service

209